With the development of modern industrial engineering technology, increasing demands of multifunctional materials drive the exploration of new applications of electrical conductive polymer nanocomposites (CPNCs). Toward applications of smart materials, sensing performance of CPNCs has gained immense attention in the last decade. Among them, strain sensors, based on piezoresistive behavior of CPNCs, are of high potential to carry out structural health monitoring (SHM) tasks. Poly(vinylidene fluoride) (PVDF) is highly thought to be potential for SHM applications in civil infrastructures like bridges and railway systems, mechanical systems, automobiles, windgenetors and airplanes, etc. because of its combination of flexibility, low weight, low thermal conductivity, high chemical corrosion resistance, and heat resistance, etc.
This work aimed to achieve high piezoresistive sensitivity and wide measurable strain ranges in carbon nanotube based poly(vinylidene fluoride) (PVDF) nanocomposites. Four strategies were introduced to tune the sensitivity of the relative electrical resistance change (ΔR/R0) versus the applied tensile strain for such nanocomposites. Issues like the influence of dispersion of multi-walled carbon nanotubes (MWCNTs) on initial resistivity of PVDF nanocomposites and conductive network structure of MWCNTs, as well as piezoresistive properties of the nanocomposites, were addressed when using differently functionalized MWCNTs (strategy 1).
In addition, the effects of crystalline phases of PVDF, mechanical ductility of its nanocomposites and interfacial interactions between PVDF and fillers on piezoresistive properties of PVDF nanocomposites were studied. Using hybrid fillers, to combine MWCNTs with conductive carbon black (strategy 2) or isolating organoclay (strategy 3), piezoresistive sensitivity and sensing strain ranges of PVDF nanocomposites could be tuned. Besides, both higher sensitivity and larger measurable strain ranges are achieved simultaneously in PVDF/MWCNT nanocomposites when using the ionic liquid (IL) BMIM+PF6- as interface linker/modifier (strategy 4).
The detailed results and highlights are summarized as following:
1. The surface functionalization of MWCNTs influences their dispersion in the PVDF matrix, the PVDF-nanotube interactions and crystalline phases of PVDF, which finally results in different ΔR/R0 and the strain at the yield point (possibly the upper limit of sensing strain ranges). As a whole, regarding to the fabrication of strain sensors based on PVDF/MWCNT nanocomposite, in contrast to pristine CNTs, CNTs-COOH and CNTs-OH, CNT-NH2 filled PVDF nanocomposites possess not only high piezoresistive sensitivity but also wide measurable strain ranges. Gauge factor, i.e. GF, is ca.14 at 10% strain (strain at the yield point) for the nanocomposites containing 0.75% CNTs-NH2.
2. Using hybrid fillers of CNTs and CB to construct strain-susceptible network structure (conductive pathway consisting of string-like array of CNTs and CB particles) enhances the piezoresistive sensitivity of PVDF nanocomposites, which is tightly associated with the CNT content in hybrid fillers and mCNTs/mCB. The best piezoresistive effect is achieved in PVDF nanocomposites with fixed CNT content lower than the ΦC (0.53 wt. %) of PVDF/CNT nanocomposites.
3. ΔR/R0 and possible sensing strain ranges of PVDF nanocomposites were tailored by changing crystalline phases of PVDF and PVDF-MWCNT interactions. Besides, the increase of the strain at yield point in PVDF nanocomposites filled by CNTs-OH is more obvious than that in the nanocomposites containing the same amount of clay and CNTs. The nanocomposite consisting of 0.25% clay and 0.75% CNTs-OH have ca. 70% increase of the strain at the yield point (17%) and the GF at this strain is ca. 14, while GF for the nanocomposite filled by only 0.75% CNTs-OH is ca. 5 at 10% strain.
4. IL BMIM+PF6- served as interface linker for PVDF and MWCNTs, which significantly increased the values of ΔR/R0 and strain at the yield point of PVDF nanocomposites simultaneously. Besides, this increases with increasing IL content. With the aid of IL, the dispersion of nanotube and toughness of the nanocomposites are greatly improved, but the electrical conductivity of the nanocomposites is decreased with the incorporation of IL, which is related to the IL modified PVDF-MWCNT interface connection or bonding. GF reaches ca. 60 at 21% strain (the strain at the yield point) for PVDF nanocomposites filled by 10% IL premixed 2%CNTs-COOH.
Identifer | oai:union.ndltd.org:DRESDEN/oai:qucosa.de:bsz:14-qucosa-201959 |
Date | 21 April 2016 |
Creators | Ke, Kai |
Contributors | Technische Universität Dresden, Fakultät Mathematik und Naturwissenschaften, Prof. Dr. Brigitte Voit, Prof. Dr. Brigitte Voit, Prof. Dr. Karl Schulte |
Publisher | Saechsische Landesbibliothek- Staats- und Universitaetsbibliothek Dresden |
Source Sets | Hochschulschriftenserver (HSSS) der SLUB Dresden |
Language | English |
Detected Language | English |
Type | doc-type:doctoralThesis |
Format | application/pdf |
Page generated in 0.0022 seconds