The main goal of this study consists of the development of new asphalt mixes, based on industrial waste materials as replacement of natural aggregates. To achieve this purpose, a new characterisation of these pavements was proposed so to verify that the new mix has good mechanical performance without any detrimental impact to the environment.
This characterisation was divided in three distinct steps:
• a physical and chemical characterisation of the different constituents of asphalt concrete, as well the natural materials as the industrial waste considered as potentially secondary aggregates,
• a study of the bitumen-aggregate interface by means of two techniques: a qualitative method (scanning electron microscope) and a quantitative one (nanoindentation)
• an evaluation of the mechanical performance of mixes containing industrial waste, before and after recycling, by means of four standard road-engineering tests.
The numerous results allowed to put in evidence the possibility to reuse some industrial waste materials in asphalt concrete. In addition, this characterisation containing both chemical and mechanical aspects, at the microscopic and macroscopic scales, would permit the transposition of this study to the whole of asphalt concrete./
Le principal objectif de ce travail consiste en le développement de nouveaux mélanges bitumineux utilisant des déchets industriels en tant que remplacement des matériaux naturels. Pour ce faire, une nouvelle caractérisation de ces revêtements a été proposée afin de vérifier que le nouveau revêtement obtenu présente de bonnes performances mécaniques tout en évitant un impact environnemental néfaste.
Cette caractérisation a été scindée en trois étapes distinctes :
• une caractérisation physique et chimique des différents constituants de l’enrobé bitumineux, à savoir les granulats naturels mais également les déchets industriels, candidats en tant que matériaux secondaires,
• une étude de l’interface bitume-granulat et ce, au moyen de deux techniques : une méthode qualitative (microscope électronique à balayage)et une méthode quantitative (nanoindentation),
• une évaluation des performances mécaniques des mélanges comportant des déchets industriels avant et après recyclage et ce, au moyen de quatre tests usuels de l’ingénierie routière.
Les nombreux résultats obtenus ont permis de mettre en évidence la possibilité de valoriser certains déchets industriels dans les enrobés bitumineux. De plus, la mise en place d’une caractérisation comportant des aspects chimiques et mécaniques, à la fois à l’échelle microscopique et macroscopique, permettra la transposition de cette étude à l’ensemble des enrobés bitumineux.
Identifer | oai:union.ndltd.org:BICfB/oai:ulb.ac.be:ETDULB:ULBetd-02062007-092717 |
Date | 26 February 2007 |
Creators | Nguyen, Pham Quynh Yên PQY |
Contributors | Delplancke, Marie-Paule, Segers, Luc, Verbrugge, Jean-Claude, Godet, Stéphane, Van Rooten, Claude, Molenaar, André |
Publisher | Universite Libre de Bruxelles |
Source Sets | Bibliothèque interuniversitaire de la Communauté française de Belgique |
Language | English |
Detected Language | French |
Type | text |
Format | application/pdf |
Source | http://theses.ulb.ac.be/ETD-db/collection/available/ULBetd-02062007-092717/ |
Rights | mixed, J'accepte que le texte de la thèse (ci-après l'oeuvre), sous réserve des parties couvertes par la confidentialité, soit publié dans le recueil électronique des thèses ULB. A cette fin, je donne licence à ULB : - le droit de fixer et de reproduire l'oeuvre sur support électronique : logiciel ETD/db - le droit de communiquer l'oeuvre au public Cette licence, gratuite et non exclusive, est valable pour toute la durée de la propriété littéraire et artistique, y compris ses éventuelles prolongations, et pour le monde entier. Je conserve tous les autres droits pour la reproduction et la communication de la thèse, ainsi que le droit de l'utiliser dans de futurs travaux. Je certifie avoir obtenu, conformément à la législation sur le droit d'auteur et aux exigences du droit à l'image, toutes les autorisations nécessaires à la reproduction dans ma thèse d'images, de textes, et/ou de toute oeuvre protégés par le droit d'auteur, et avoir obtenu les autorisations nécessaires à leur communication à des tiers. Au cas où un tiers est titulaire d'un droit de propriété intellectuelle sur tout ou partie de ma thèse, je certifie avoir obtenu son autorisation écrite pour l'exercice des droits mentionnés ci-dessus. |
Page generated in 0.0014 seconds