{"id":{"repo_id":"buffalo","oai_identifier":"oai:ubir.buffalo.edu:10477/87747"},"canonical_url":"https://search.ndltd.org/etd/buffalo/oai:ubir.buffalo.edu:10477/87747","repository":{"repo_id":"buffalo","name":"Buffalo","base_url":"https://ubir.buffalo.edu/oai/request"},"display":{"title":"Effect of Connector Design on the Failure Strength of Implant-Supported Posterior 3-Unit Yttrium Tetragonal Zirconia Polycrystal (4Y-TZP) Fixed Dental Prosthesis","abstract":"Objectives: The purpose of this in vitro study was to evaluate the relationship between the embrasure design and the fracture resistance of 3-unit implant-supported mandibular posterior fixed dental prosthesis (FDP) made of yttrium tetragonal zirconia polycrystal (Y-TZP) after clinical simulation with low-temperature degradation (LTD).Methods: A mandibular implant-supported 3-unit FDP on mandibular second premolar and second molar was generated using a CAD system. Subsequently, The FDP design was modified to create separate specimens with 0.5 mm and 1.0 mm diameter gingival embrasure. Ten FPDs with the 0.5 mm gingival embrasure and twenty FDPs with the 1.0 mm gingival embrasure were fabricated from 4Y-TZP discs with a CNC dental milling machine. Before sintering, ten FDPs of the 1.0 mm group underwent further disc separation at the gingival embrasures. After sintering, all thirty zirconia FDPs were subjected to an accelerated aging process, LTD (121 °C steam at 2 bar for 13.5 h). A static load-bearing test was then performed with a universal testing machine (MTS mini Bionix 2) to measure the maximum failure load. Data were analyzed using a one-way ANOVA, with a significance level of 0.05.Results: One-way ANOVA indicated a statistically significant difference between the groups (p < 0.05). Overall, the 0.5mm gingival embrasure group showed the highest failure load (1143.9 ± 161.2 N), and the 1.0mm gingival embrasure with disc separation group exhibited the lowest failure load (796.6 ± 192.9 N). Pair-wise tests with Tukey HSD revealed that the 1.0 mm gingival embrasure with disc separation group showed a significantly lower maximum failure load compared to the maximum failure load found in the 0.5 mm gingival embrasure group and the 1.0 mm gingival embrasure group. There was no statistically significant difference in failure strength between the 0.5mm gingival embrasure group and the 1.0 mm gingival embrasure group. The majority of the fractured specimens indicated a consistent fracture pattern initiated from the gingival embrasure and extended towards the pontic's occlusal surface. Conclusion: Within the limitation of this study, the following conclusions could be drawn: 1. Disc separation at the gingival embrasure before sintering significantly reduces the fracture resistance of 4Y-TZP 3-unit implant-supported mandibular posterior FDPs. 2. Given that the other parameters of the FDPs remain identical, modifying the gingival embrasure diameter from 1.0 mm to 0.5 mm does not significantly decrease the failure strength of the restoration.","abstract_html":"Objectives: The purpose of this in vitro study was to evaluate the relationship between the embrasure design and the fracture resistance of 3-unit implant-supported mandibular posterior fixed dental prosthesis (FDP) made of yttrium tetragonal zirconia polycrystal (Y-TZP) after clinical simulation with low-temperature degradation (LTD).Methods: A mandibular implant-supported 3-unit FDP on mandibular second premolar and second molar was generated using a CAD system. Subsequently, The FDP design was modified to create separate specimens with 0.5 mm and 1.0 mm diameter gingival embrasure. Ten FPDs with the 0.5 mm gingival embrasure and twenty FDPs with the 1.0 mm gingival embrasure were fabricated from 4Y-TZP discs with a CNC dental milling machine. Before sintering, ten FDPs of the 1.0 mm group underwent further disc separation at the gingival embrasures. After sintering, all thirty zirconia FDPs were subjected to an accelerated aging process, LTD (121 °C steam at 2 bar for 13.5 h). A static load-bearing test was then performed with a universal testing machine (MTS mini Bionix 2) to measure the maximum failure load. Data were analyzed using a one-way ANOVA, with a significance level of 0.05.Results: One-way ANOVA indicated a statistically significant difference between the groups (p &lt; 0.05). Overall, the 0.5mm gingival embrasure group showed the highest failure load (1143.9 ± 161.2 N), and the 1.0mm gingival embrasure with disc separation group exhibited the lowest failure load (796.6 ± 192.9 N). Pair-wise tests with Tukey HSD revealed that the 1.0 mm gingival embrasure with disc separation group showed a significantly lower maximum failure load compared to the maximum failure load found in the 0.5 mm gingival embrasure group and the 1.0 mm gingival embrasure group. There was no statistically significant difference in failure strength between the 0.5mm gingival embrasure group and the 1.0 mm gingival embrasure group. The majority of the fractured specimens indicated a consistent fracture pattern initiated from the gingival embrasure and extended towards the pontic&#x27;s occlusal surface. Conclusion: Within the limitation of this study, the following conclusions could be drawn: 1. Disc separation at the gingival embrasure before sintering significantly reduces the fracture resistance of 4Y-TZP 3-unit implant-supported mandibular posterior FDPs. 2. Given that the other parameters of the FDPs remain identical, modifying the gingival embrasure diameter from 1.0 mm to 0.5 mm does not significantly decrease the failure strength of the restoration.","abstract_has_math":false,"creators":["Lin, Yu Chun"],"institution":"State University of New York at Buffalo","degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":null,"school":null,"contributors":["Kim, Hyeongil","Oral Sciences"],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2021,"date_issued":"2021","date_published":"2021","updated_at":"2026-11-19T07:10:06Z","subjects":["dentistry","materials science"],"languages":["eng"],"rights":["Copyright retained by author.","Users of works found in University at Buffalo Institutional Repository (UBIR) are responsible for identifying and contacting the copyright owner for permission to reuse. University at Buffalo Libraries do not manage rights for copyright-protected works and cannot assist with permissions."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"https://hdl.handle.net/10477/87747","outbound_label":"Handle","outbound_source":"dc:identifier","record_url":"https://hdl.handle.net/10477/87747","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Abuffalo%3Aoai%3Aubir.buffalo.edu%3A10477%2F87747","prefix":"oai_dc"},"source_record":{"url":"https://ubir.buffalo.edu/oai/request?verb=GetRecord&metadataPrefix=qdc&identifier=oai%3Aubir.buffalo.edu%3A10477%2F87747","prefix":"qdc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor","label":"Contributor","values":["Kim, Hyeongil","Oral Sciences"]},{"key":"dc:creator","label":"Author","values":["Lin, Yu Chun"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2025-06-09T15:18:18Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2025-06-09T15:18:18Z"]},{"key":"dc:date.created","label":"Dc Date Created","values":["2025-06-09T15:18:18Z"]},{"key":"dc:date.issued","label":"Date","values":["2021"]},{"key":"dc:publisher","label":"Institution","values":["State University of New York at Buffalo"]},{"key":"dc:type","label":"Dc Type","values":["Text","Thesis"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["dentistry","materials science"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["eng"]},{"key":"dc:rights","label":"Dc Rights","values":["Copyright retained by author.","Users of works found in University at Buffalo Institutional Repository (UBIR) are responsible for identifying and contacting the copyright owner for permission to reuse. University at Buffalo Libraries do not manage rights for copyright-protected works and cannot assist with permissions."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://hdl.handle.net/10477/87747"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Objectives: The purpose of this in vitro study was to evaluate the relationship between the embrasure design and the fracture resistance of 3-unit implant-supported mandibular posterior fixed dental prosthesis (FDP) made of yttrium tetragonal zirconia polycrystal (Y-TZP) after clinical simulation with low-temperature degradation (LTD).Methods: A mandibular implant-supported 3-unit FDP on mandibular second premolar and second molar was generated using a CAD system. Subsequently, The FDP design was modified to create separate specimens with 0.5 mm and 1.0 mm diameter gingival embrasure. Ten FPDs with the 0.5 mm gingival embrasure and twenty FDPs with the 1.0 mm gingival embrasure were fabricated from 4Y-TZP discs with a CNC dental milling machine. Before sintering, ten FDPs of the 1.0 mm group underwent further disc separation at the gingival embrasures. After sintering, all thirty zirconia FDPs were subjected to an accelerated aging process, LTD (121 °C steam at 2 bar for 13.5 h). A static load-bearing test was then performed with a universal testing machine (MTS mini Bionix 2) to measure the maximum failure load. Data were analyzed using a one-way ANOVA, with a significance level of 0.05.Results: One-way ANOVA indicated a statistically significant difference between the groups (p < 0.05). Overall, the 0.5mm gingival embrasure group showed the highest failure load (1143.9 ± 161.2 N), and the 1.0mm gingival embrasure with disc separation group exhibited the lowest failure load (796.6 ± 192.9 N). Pair-wise tests with Tukey HSD revealed that the 1.0 mm gingival embrasure with disc separation group showed a significantly lower maximum failure load compared to the maximum failure load found in the 0.5 mm gingival embrasure group and the 1.0 mm gingival embrasure group. There was no statistically significant difference in failure strength between the 0.5mm gingival embrasure group and the 1.0 mm gingival embrasure group. The majority of the fractured specimens indicated a consistent fracture pattern initiated from the gingival embrasure and extended towards the pontic's occlusal surface. Conclusion: Within the limitation of this study, the following conclusions could be drawn: 1. Disc separation at the gingival embrasure before sintering significantly reduces the fracture resistance of 4Y-TZP 3-unit implant-supported mandibular posterior FDPs. 2. Given that the other parameters of the FDPs remain identical, modifying the gingival embrasure diameter from 1.0 mm to 0.5 mm does not significantly decrease the failure strength of the restoration.","**To request an accessible version of the file(s) associated with this item, contact library@buffalo.edu. Please include the item's persistent URL [http://hdl.handle.net/. . .] in your request.**"]},{"key":"dc:title","label":"Title","values":["Effect of Connector Design on the Failure Strength of Implant-Supported Posterior 3-Unit Yttrium Tetragonal Zirconia Polycrystal (4Y-TZP) Fixed Dental Prosthesis"]}]}],"canonical_facts":{"dc:contributor":["Kim, Hyeongil","Oral Sciences"],"dc:creator":["Lin, Yu Chun"],"dc:date":["2025-06-09T15:18:18Z"],"dc:date.available":["2025-06-09T15:18:18Z"],"dc:date.created":["2025-06-09T15:18:18Z"],"dc:date.issued":["2021"],"dc:description.abstract":["Objectives: The purpose of this in vitro study was to evaluate the relationship between the embrasure design and the fracture resistance of 3-unit implant-supported mandibular posterior fixed dental prosthesis (FDP) made of yttrium tetragonal zirconia polycrystal (Y-TZP) after clinical simulation with low-temperature degradation (LTD).Methods: A mandibular implant-supported 3-unit FDP on mandibular second premolar and second molar was generated using a CAD system. Subsequently, The FDP design was modified to create separate specimens with 0.5 mm and 1.0 mm diameter gingival embrasure. Ten FPDs with the 0.5 mm gingival embrasure and twenty FDPs with the 1.0 mm gingival embrasure were fabricated from 4Y-TZP discs with a CNC dental milling machine. Before sintering, ten FDPs of the 1.0 mm group underwent further disc separation at the gingival embrasures. After sintering, all thirty zirconia FDPs were subjected to an accelerated aging process, LTD (121 °C steam at 2 bar for 13.5 h). A static load-bearing test was then performed with a universal testing machine (MTS mini Bionix 2) to measure the maximum failure load. Data were analyzed using a one-way ANOVA, with a significance level of 0.05.Results: One-way ANOVA indicated a statistically significant difference between the groups (p < 0.05). Overall, the 0.5mm gingival embrasure group showed the highest failure load (1143.9 ± 161.2 N), and the 1.0mm gingival embrasure with disc separation group exhibited the lowest failure load (796.6 ± 192.9 N). Pair-wise tests with Tukey HSD revealed that the 1.0 mm gingival embrasure with disc separation group showed a significantly lower maximum failure load compared to the maximum failure load found in the 0.5 mm gingival embrasure group and the 1.0 mm gingival embrasure group. There was no statistically significant difference in failure strength between the 0.5mm gingival embrasure group and the 1.0 mm gingival embrasure group. The majority of the fractured specimens indicated a consistent fracture pattern initiated from the gingival embrasure and extended towards the pontic's occlusal surface. Conclusion: Within the limitation of this study, the following conclusions could be drawn: 1. Disc separation at the gingival embrasure before sintering significantly reduces the fracture resistance of 4Y-TZP 3-unit implant-supported mandibular posterior FDPs. 2. Given that the other parameters of the FDPs remain identical, modifying the gingival embrasure diameter from 1.0 mm to 0.5 mm does not significantly decrease the failure strength of the restoration.","**To request an accessible version of the file(s) associated with this item, contact library@buffalo.edu. Please include the item's persistent URL [http://hdl.handle.net/. . .] in your request.**"],"dc:identifier":["http://hdl.handle.net/10477/87747"],"dc:language":["eng"],"dc:publisher":["State University of New York at Buffalo"],"dc:rights":["Copyright retained by author.","Users of works found in University at Buffalo Institutional Repository (UBIR) are responsible for identifying and contacting the copyright owner for permission to reuse. University at Buffalo Libraries do not manage rights for copyright-protected works and cannot assist with permissions."],"dc:subject":["dentistry","materials science"],"dc:title":["Effect of Connector Design on the Failure Strength of Implant-Supported Posterior 3-Unit Yttrium Tetragonal Zirconia Polycrystal (4Y-TZP) Fixed Dental Prosthesis"],"dc:type":["Text","Thesis"]},"updated_at":"2026-11-19T07:10:06Z"}