{"id":{"repo_id":"durham","oai_identifier":"oai:etheses.durham.ac.uk:8284"},"canonical_url":"https://search.ndltd.org/etd/durham/oai:etheses.durham.ac.uk:8284","repository":{"repo_id":"durham","name":"Durham University","base_url":"http://etheses.dur.ac.uk/cgi/oai2"},"display":{"title":"Electrical properties of hot-pressed nitrogen ceramics","abstract":"Some electrical properties of hot-pressed Si(_3)N(_4), 5 W/o MgO/Si(_3)N(_4) and two sialons, Si(_6-z). Al(_z).O(_z).N(_8-z) having Z = 3.2 and Z = 4.0 have been measured, using a variety of techniques, between 18 c and l000 C. The electrical behaviour of all the materials showed similar general features. The d.c. conductivities were in the range of 10(^-15)-10(^-16)Ω(^-1)cm(^-1) at 18 C and rose to 10(^-6)-10(^-5)Ω(^-1)cm(^-1) at 1000 C. The current density-field (J3-E) characteristics were ohmic in applied fields of less than 3 x 10(^3) volt cm(^-1), conductivity increased with electric field above that range. Above about 280 C, o(_dc) was independent of E, its temperature dependence following log o(_dc) aT(^-1). Below about 230 c conductivity fitted a o α exp ((^-B/)T(^1/4)) law in both low and high fields. The activation energies were in the range of 1.45-1.80 eV and 0.05-0.15 eV at above 300 C and near room temperatures respectively. Time dependent charging (I(_C)) and discharging (I(_D) currents were observed which followed a I(t)α t(^-n) law with n = 0.7-0.8 at room temperature. The exponent n for I(_C) decreased with increasing temperature. Hall effect and thermoelectric power measurements enabled the Hall mobility to be estimated as less than 10(^-4) cm(^2)v(^-1)sec(^-1) at above 400 C and showed that the materials were all p-type between 400 and 900 C and n-type above 900 C. The drift mobility obtained from observations of transit time effects was 1 x 10(^-8)-5 x 10(^-9) cm(^2)v(^-1)sec(^-1). Various hopping models to explain the data are considered. At room temperature the variation of conductivity (o’ (w) α w(^n) with frequency over the range 200 Hz to 9.3 GHz followed the o’(w) α w(^n) law with n = 0.9. The dielectric constant (Σ') and loss (tano) both fell slightly over this frequency range, the average values at 10(^5) Hz being about 9.5 and 5 X 10(^-3) respectively. At temperatures up to 500 C the data fits well with the 'Universal dielectric law' Σ\"(w) α w(^n-1) and approximately fits the Kramers-Kronig relation Σ\"(w)/(_Σ’(w) – Σ). = cot ((^nπ)/(_2)) with 0.5 < n < 1. The exponent n decreases with increasing temperature. The effects may be caused by either non-Debye dipolar or hopping charge phenomena. Similar studies of electrical properties for 30 m/o Li-sialon and 14.3 m/o Y-sialon were also made in an attempt to relate the electrical properties and compositions of pure and doped sialons.","abstract_html":"Some electrical properties of hot-pressed Si(_3)N(_4), 5 W/o MgO/Si(_3)N(_4) and two sialons, Si(_6-z). Al(_z).O(_z).N(_8-z) having Z = 3.2 and Z = 4.0 have been measured, using a variety of techniques, between 18 c and l000 C. The electrical behaviour of all the materials showed similar general features. The d.c. conductivities were in the range of 10(^-15)-10(^-16)Ω(^-1)cm(^-1) at 18 C and rose to 10(^-6)-10(^-5)Ω(^-1)cm(^-1) at 1000 C. The current density-field (J3-E) characteristics were ohmic in applied fields of less than 3 x 10(^3) volt cm(^-1), conductivity increased with electric field above that range. Above about 280 C, o(_dc) was independent of E, its temperature dependence following log o(_dc) aT(^-1). Below about 230 c conductivity fitted a o α exp ((^-B/)T(^1/4)) law in both low and high fields. The activation energies were in the range of 1.45-1.80 eV and 0.05-0.15 eV at above 300 C and near room temperatures respectively. Time dependent charging (I(_C)) and discharging (I(_D) currents were observed which followed a I(t)α t(^-n) law with n = 0.7-0.8 at room temperature. The exponent n for I(_C) decreased with increasing temperature. Hall effect and thermoelectric power measurements enabled the Hall mobility to be estimated as less than 10(^-4) cm(^2)v(^-1)sec(^-1) at above 400 C and showed that the materials were all p-type between 400 and 900 C and n-type above 900 C. The drift mobility obtained from observations of transit time effects was 1 x 10(^-8)-5 x 10(^-9) cm(^2)v(^-1)sec(^-1). Various hopping models to explain the data are considered. At room temperature the variation of conductivity (o’ (w) α w(^n) with frequency over the range 200 Hz to 9.3 GHz followed the o’(w) α w(^n) law with n = 0.9. The dielectric constant (Σ&#x27;) and loss (tano) both fell slightly over this frequency range, the average values at 10(^5) Hz being about 9.5 and 5 X 10(^-3) respectively. At temperatures up to 500 C the data fits well with the &#x27;Universal dielectric law&#x27; Σ&quot;(w) α w(^n-1) and approximately fits the Kramers-Kronig relation Σ&quot;(w)/(_Σ’(w) – Σ). = cot ((^nπ)/(_2)) with 0.5 &lt; n &lt; 1. The exponent n decreases with increasing temperature. The effects may be caused by either non-Debye dipolar or hopping charge phenomena. Similar studies of electrical properties for 30 m/o Li-sialon and 14.3 m/o Y-sialon were also made in an attempt to relate the electrical properties and compositions of pure and doped sialons.","abstract_has_math":false,"creators":["Sharif, Rafiqul Aslam"],"institution":"Durham University","degree_name":"PhD","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":1977,"date_issued":"1977","date_published":"1977","updated_at":"2026-11-26T03:56:42Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["UkUDh:CyT"],"render_values":[{"text":"UkUDh:CyT","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":"https://etheses.durham.ac.uk/id/eprint/8284/","outbound_label":"Repository record","outbound_source":"dc:identifier.uri","record_url":"https://etheses.durham.ac.uk/id/eprint/8284/","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Adurham%3Aoai%3Aetheses.durham.ac.uk%3A8284","prefix":"oai_dc"},"source_record":{"url":"http://etheses.dur.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.durham.ac.uk%3A8284","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:creator","label":"Author","values":["Sharif, Rafiqul Aslam"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["1977"]},{"key":"dc:date.issued","label":"Date","values":["1977"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Physics, Department of","Applied Physics and Electronics"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["Durham University"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["PhD"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["UkUDh:CyT"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.durham.ac.uk/id/eprint/8284/"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Some electrical properties of hot-pressed Si(_3)N(_4), 5 W/o MgO/Si(_3)N(_4) and two sialons, Si(_6-z). Al(_z).O(_z).N(_8-z) having Z = 3.2 and Z = 4.0 have been measured, using a variety of techniques, between 18 c and l000 C. The electrical behaviour of all the materials showed similar general features. The d.c. conductivities were in the range of 10(^-15)-10(^-16)Ω(^-1)cm(^-1) at 18 C and rose to 10(^-6)-10(^-5)Ω(^-1)cm(^-1) at 1000 C. The current density-field (J3-E) characteristics were ohmic in applied fields of less than 3 x 10(^3) volt cm(^-1), conductivity increased with electric field above that range. Above about 280 C, o(_dc) was independent of E, its temperature dependence following log o(_dc) aT(^-1). Below about 230 c conductivity fitted a o α exp ((^-B/)T(^1/4)) law in both low and high fields. The activation energies were in the range of 1.45-1.80 eV and 0.05-0.15 eV at above 300 C and near room temperatures respectively. Time dependent charging (I(_C)) and discharging (I(_D) currents were observed which followed a I(t)α t(^-n) law with n = 0.7-0.8 at room temperature. The exponent n for I(_C) decreased with increasing temperature. Hall effect and thermoelectric power measurements enabled the Hall mobility to be estimated as less than 10(^-4) cm(^2)v(^-1)sec(^-1) at above 400 C and showed that the materials were all p-type between 400 and 900 C and n-type above 900 C. The drift mobility obtained from observations of transit time effects was 1 x 10(^-8)-5 x 10(^-9) cm(^2)v(^-1)sec(^-1). Various hopping models to explain the data are considered. At room temperature the variation of conductivity (o’ (w) α w(^n) with frequency over the range 200 Hz to 9.3 GHz followed the o’(w) α w(^n) law with n = 0.9. The dielectric constant (Σ') and loss (tano) both fell slightly over this frequency range, the average values at 10(^5) Hz being about 9.5 and 5 X 10(^-3) respectively. At temperatures up to 500 C the data fits well with the 'Universal dielectric law' Σ\"(w) α w(^n-1) and approximately fits the Kramers-Kronig relation Σ\"(w)/(_Σ’(w) – Σ). = cot ((^nπ)/(_2)) with 0.5 < n < 1. The exponent n decreases with increasing temperature. The effects may be caused by either non-Debye dipolar or hopping charge phenomena. Similar studies of electrical properties for 30 m/o Li-sialon and 14.3 m/o Y-sialon were also made in an attempt to relate the electrical properties and compositions of pure and doped sialons."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Electrical properties of hot-pressed nitrogen ceramics"]}]}],"canonical_facts":{"dc:creator":["Sharif, Rafiqul Aslam"],"dc:date":["1977"],"dc:date.issued":["1977"],"dc:description.abstract":["Some electrical properties of hot-pressed Si(_3)N(_4), 5 W/o MgO/Si(_3)N(_4) and two sialons, Si(_6-z). Al(_z).O(_z).N(_8-z) having Z = 3.2 and Z = 4.0 have been measured, using a variety of techniques, between 18 c and l000 C. The electrical behaviour of all the materials showed similar general features. The d.c. conductivities were in the range of 10(^-15)-10(^-16)Ω(^-1)cm(^-1) at 18 C and rose to 10(^-6)-10(^-5)Ω(^-1)cm(^-1) at 1000 C. The current density-field (J3-E) characteristics were ohmic in applied fields of less than 3 x 10(^3) volt cm(^-1), conductivity increased with electric field above that range. Above about 280 C, o(_dc) was independent of E, its temperature dependence following log o(_dc) aT(^-1). Below about 230 c conductivity fitted a o α exp ((^-B/)T(^1/4)) law in both low and high fields. The activation energies were in the range of 1.45-1.80 eV and 0.05-0.15 eV at above 300 C and near room temperatures respectively. Time dependent charging (I(_C)) and discharging (I(_D) currents were observed which followed a I(t)α t(^-n) law with n = 0.7-0.8 at room temperature. The exponent n for I(_C) decreased with increasing temperature. Hall effect and thermoelectric power measurements enabled the Hall mobility to be estimated as less than 10(^-4) cm(^2)v(^-1)sec(^-1) at above 400 C and showed that the materials were all p-type between 400 and 900 C and n-type above 900 C. The drift mobility obtained from observations of transit time effects was 1 x 10(^-8)-5 x 10(^-9) cm(^2)v(^-1)sec(^-1). Various hopping models to explain the data are considered. At room temperature the variation of conductivity (o’ (w) α w(^n) with frequency over the range 200 Hz to 9.3 GHz followed the o’(w) α w(^n) law with n = 0.9. The dielectric constant (Σ') and loss (tano) both fell slightly over this frequency range, the average values at 10(^5) Hz being about 9.5 and 5 X 10(^-3) respectively. At temperatures up to 500 C the data fits well with the 'Universal dielectric law' Σ\"(w) α w(^n-1) and approximately fits the Kramers-Kronig relation Σ\"(w)/(_Σ’(w) – Σ). = cot ((^nπ)/(_2)) with 0.5 < n < 1. The exponent n decreases with increasing temperature. The effects may be caused by either non-Debye dipolar or hopping charge phenomena. Similar studies of electrical properties for 30 m/o Li-sialon and 14.3 m/o Y-sialon were also made in an attempt to relate the electrical properties and compositions of pure and doped sialons."],"dc:format":["text"],"dc:identifier.grantnumber":["UkUDh:CyT"],"dc:identifier.uri":["https://etheses.durham.ac.uk/id/eprint/8284/"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Physics, Department of","Applied Physics and Electronics"],"dc:publisher.institution":["Durham University"],"dcterms:accessrights":["public"],"dc:title":["Electrical properties of hot-pressed nitrogen ceramics"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["PhD"]},"updated_at":"2026-11-26T03:56:42Z"}