{"id":{"repo_id":"fu-berlin","oai_identifier":"oai:refubium.fu-berlin.de:fub188/51963"},"canonical_url":"https://search.ndltd.org/etd/fu-berlin/oai:refubium.fu-berlin.de:fub188/51963","repository":{"repo_id":"fu-berlin","name":"Freie Universität Berlin","base_url":"https://refubium.fu-berlin.de/oai/request"},"display":{"title":"Enhancing the biocompatibility of PEEK implants through O2/H2 plasma treatment: Effects on surface properties and cell behavior","abstract":"Polyetheretherketone (PEEK) has gained attention as a biomaterial in clinical applications due to its excellent mechanical properties, radiolucency, and chemical stability. However, its biologically inert surface limits direct integration with surrounding tissues, thereby constraining its broader clinical use. This study aimed to investigate the effects of low- pressure hydrogen–oxygen (H₂/O₂, 1:1) plasma surface modification on the physicochemical characteristics and biological performance of PEEK, to enhance both soft and hard tissue responses. A total of 276 PEEK specimens were fabricated and subjected to varying durations of H₂/O₂ low-pressure plasma treatment. Surface wettability, roughness, micro hardness, and chemical composition before and after treatment were assessed using water contact angle (WCA) measurements, optical profilometry, micro hardness testing, scanning electron microscopy (SEM), and X-ray photoelectron spectroscopy (XPS). The aging behavior of plasma-modified surfaces was monitored over 21 days. In vitro biological responses were evaluated using human gingival fibroblasts (iHGFs) and osteoblast-like Saos-2 cells. Soft tissue cell behavior was assessed via live/dead staining, SEM imaging, and proliferation assays, while osteogenic differentiation was evaluated through alkaline phosphatase (ALP) activity and Alizarin Red S staining. The results demonstrated that plasma treatment significantly enhanced surface wettability, reducing the WCA from 75.72° to nearly 0°, primarily due to the incorporation of oxygen-containing functional groups (C–O, C=O). Although surface hydrophilicity declined over time as a result of aging, it was better preserved in specimens treated for 15 minutes. Plasma treatment also led to a time-dependent increase in micro hardness. While surface roughness changes were minor and not statistically significant, longer treatment durations showed a trend toward increased surface etching. Biologically, plasma-modified surfaces promoted improved cell adhesion, spreading, and proliferation. Notably, the 4-minute treatment group exhibited the most favourable outcomes in terms of ALP activity and calcium deposition, surpassing even the 15-minute group. These results suggest that moderate plasma exposure can achieve optimal surface activation while avoiding the potential adverse effects of excessive oxidation, such as protein denaturation. The findings further emphasize that surface chemistry, rather than roughness, plays a dominant role in modulating cell behavior. In conclusion, H₂/O₂ low-pressure plasma treatment effectively enhances the surface properties and biological functionality of PEEK. A 4-minute treatment duration appears to offer the optimal balance for promoting favourable responses from both soft and hard tissue cells, highlighting its clinical potential in dental and orthopaedic implant applications. Nevertheless, further investigations are warranted to evaluate antimicrobial properties, gene and protein expression profiles, and in vivo osseointegration outcomes.","abstract_html":"Polyetheretherketone (PEEK) has gained attention as a biomaterial in clinical applications due to its excellent mechanical properties, radiolucency, and chemical stability. However, its biologically inert surface limits direct integration with surrounding tissues, thereby constraining its broader clinical use. This study aimed to investigate the effects of low- pressure hydrogen–oxygen (H₂/O₂, 1:1) plasma surface modification on the physicochemical characteristics and biological performance of PEEK, to enhance both soft and hard tissue responses. A total of 276 PEEK specimens were fabricated and subjected to varying durations of H₂/O₂ low-pressure plasma treatment. Surface wettability, roughness, micro hardness, and chemical composition before and after treatment were assessed using water contact angle (WCA) measurements, optical profilometry, micro hardness testing, scanning electron microscopy (SEM), and X-ray photoelectron spectroscopy (XPS). The aging behavior of plasma-modified surfaces was monitored over 21 days. In vitro biological responses were evaluated using human gingival fibroblasts (iHGFs) and osteoblast-like Saos-2 cells. Soft tissue cell behavior was assessed via live/dead staining, SEM imaging, and proliferation assays, while osteogenic differentiation was evaluated through alkaline phosphatase (ALP) activity and Alizarin Red S staining. The results demonstrated that plasma treatment significantly enhanced surface wettability, reducing the WCA from 75.72° to nearly 0°, primarily due to the incorporation of oxygen-containing functional groups (C–O, C=O). Although surface hydrophilicity declined over time as a result of aging, it was better preserved in specimens treated for 15 minutes. Plasma treatment also led to a time-dependent increase in micro hardness. While surface roughness changes were minor and not statistically significant, longer treatment durations showed a trend toward increased surface etching. Biologically, plasma-modified surfaces promoted improved cell adhesion, spreading, and proliferation. Notably, the 4-minute treatment group exhibited the most favourable outcomes in terms of ALP activity and calcium deposition, surpassing even the 15-minute group. These results suggest that moderate plasma exposure can achieve optimal surface activation while avoiding the potential adverse effects of excessive oxidation, such as protein denaturation. The findings further emphasize that surface chemistry, rather than roughness, plays a dominant role in modulating cell behavior. In conclusion, H₂/O₂ low-pressure plasma treatment effectively enhances the surface properties and biological functionality of PEEK. A 4-minute treatment duration appears to offer the optimal balance for promoting favourable responses from both soft and hard tissue cells, highlighting its clinical potential in dental and orthopaedic implant applications. Nevertheless, further investigations are warranted to evaluate antimicrobial properties, gene and protein expression profiles, and in vivo osseointegration outcomes.","abstract_has_math":false,"creators":["Weng, Shengxin"],"institution":null,"degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":"Charité - Universitätsmedizin Berlin","school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":["N.N."],"year":2026,"date_issued":"2026","date_published":"2026","updated_at":"2026-11-19T03:53:47Z","subjects":["PEEK","Hydrogen/oxygen low-pressure plasma","Osteoconductive","Biocompatibility"],"languages":["eng"],"rights":["open access"],"rights_urls":["https://www.fu-berlin.de/sites/ub/publizieren/refubium/rechtliches/index.html"],"identifier_entries":[{"key":"dc:identifier.urn","label":"URN","values":["urn:nbn:de:kobv:188-refubium-51963-9"],"render_values":[{"text":"urn:nbn:de:kobv:188-refubium-51963-9","href":"https://nbn-resolving.org/urn:nbn:de:kobv:188-refubium-51963-9","code":true}]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://refubium.fu-berlin.de/handle/fub188/51963"],"render_values":[{"text":"https://refubium.fu-berlin.de/handle/fub188/51963","href":"https://refubium.fu-berlin.de/handle/fub188/51963","code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":"https://doi.org/10.17169/refubium-51699","outbound_label":"DOI","outbound_source":"dc:identifier.uri","record_url":"https://doi.org/10.17169/refubium-51699","record_label":"Repository record","record_kind":"doi","record_source":"dc:identifier.uri","access_status":"open","embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Afu-berlin%3Aoai%3Arefubium.fu-berlin.de%3Afub188%2F51963","prefix":"oai_dc"},"source_record":{"url":"https://refubium.fu-berlin.de/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Arefubium.fu-berlin.de%3Afub188%2F51963","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.committeemember","label":"Committee Member","values":["N.N."]},{"key":"dc:contributor.department","label":"Department","values":["Charité - Universitätsmedizin Berlin"]},{"key":"dc:creator","label":"Author","values":["Weng, Shengxin"]},{"key":"person:gender","label":"Person Gender","values":["female"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.issued","label":"Date","values":["2026"]},{"key":"dc:type","label":"Dc Type","values":["doc-type:doctoralThesis"]},{"key":"dc:type.dcmitype","label":"Dc Type Dcmitype","values":["Text"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["PEEK","Hydrogen/oxygen low-pressure plasma","Osteoconductive","Biocompatibility"]},{"key":"dc:subject.ddc","label":"Dc Subject Ddc","values":["ddc:610"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["eng"]},{"key":"dc:rights.accessrights","label":"Access Rights","values":["open access"]},{"key":"dc:rights.proquest","label":"Dc Rights Proquest","values":["accept"]},{"key":"dc:rights.uri","label":"Rights URI","values":["https://www.fu-berlin.de/sites/ub/publizieren/refubium/rechtliches/index.html"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://refubium.fu-berlin.de/handle/fub188/51963","http://dx.doi.org/10.17169/refubium-51699"]},{"key":"dc:identifier.urn","label":"URN","values":["urn:nbn:de:kobv:188-refubium-51963-9"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Polyetheretherketone (PEEK) has gained attention as a biomaterial in clinical applications due to its excellent mechanical properties, radiolucency, and chemical stability. However, its biologically inert surface limits direct integration with surrounding tissues, thereby constraining its broader clinical use. This study aimed to investigate the effects of low- pressure hydrogen–oxygen (H₂/O₂, 1:1) plasma surface modification on the physicochemical characteristics and biological performance of PEEK, to enhance both soft and hard tissue responses. A total of 276 PEEK specimens were fabricated and subjected to varying durations of H₂/O₂ low-pressure plasma treatment. Surface wettability, roughness, micro hardness, and chemical composition before and after treatment were assessed using water contact angle (WCA) measurements, optical profilometry, micro hardness testing, scanning electron microscopy (SEM), and X-ray photoelectron spectroscopy (XPS). The aging behavior of plasma-modified surfaces was monitored over 21 days. In vitro biological responses were evaluated using human gingival fibroblasts (iHGFs) and osteoblast-like Saos-2 cells. Soft tissue cell behavior was assessed via live/dead staining, SEM imaging, and proliferation assays, while osteogenic differentiation was evaluated through alkaline phosphatase (ALP) activity and Alizarin Red S staining. The results demonstrated that plasma treatment significantly enhanced surface wettability, reducing the WCA from 75.72° to nearly 0°, primarily due to the incorporation of oxygen-containing functional groups (C–O, C=O). Although surface hydrophilicity declined over time as a result of aging, it was better preserved in specimens treated for 15 minutes. Plasma treatment also led to a time-dependent increase in micro hardness. While surface roughness changes were minor and not statistically significant, longer treatment durations showed a trend toward increased surface etching. Biologically, plasma-modified surfaces promoted improved cell adhesion, spreading, and proliferation. Notably, the 4-minute treatment group exhibited the most favourable outcomes in terms of ALP activity and calcium deposition, surpassing even the 15-minute group. These results suggest that moderate plasma exposure can achieve optimal surface activation while avoiding the potential adverse effects of excessive oxidation, such as protein denaturation. The findings further emphasize that surface chemistry, rather than roughness, plays a dominant role in modulating cell behavior. In conclusion, H₂/O₂ low-pressure plasma treatment effectively enhances the surface properties and biological functionality of PEEK. A 4-minute treatment duration appears to offer the optimal balance for promoting favourable responses from both soft and hard tissue cells, highlighting its clinical potential in dental and orthopaedic implant applications. Nevertheless, further investigations are warranted to evaluate antimicrobial properties, gene and protein expression profiles, and in vivo osseointegration outcomes.","Polyetheretherketon (PEEK) hat als Biomaterial für klinische Anwendungen aufgrund seiner hervorragenden mechanischen Eigenschaften, Röntgentransparenz und chemischen Stabilität an Bedeutung gewonnen. Seine biologische Inertheit begrenzt jedoch die direkte Integration in umgebendes Gewebe, was den breiteren klinischen Einsatz einschränkt. Diese Studie untersuchte die Effekte einer Niederdruck-Wasserstoff- Sauerstoff-Plasmabehandlung (H₂/O₂, 1:1) auf die physikochemischen Eigenschaften und die biologische Performance von PEEK, um die Weich- und Hartgewebereaktionen zu verbessern. 276 PEEK-Proben wurden hergestellt und unterschiedlich langen H₂/O₂- Niederdruckplasmabehandlungen unterzogen. Oberflächenbenetzbarkeit, Rauheit, Mikrohärte und chemische Zusammensetzung vor/nach Behandlung wurden mittels Wasser-Kontaktwinkelmessungen (WCA), optischer Profilometrie, Mikrohärtetests, Rasterelektronenmikroskopie (REM) und Röntgenphotoelektronenspektroskopie (XPS) analysiert. Das Alterungsverhalten plasmamodifizierter Oberflächen wurde über 21 Tage beobachtet. Die biologischen Reaktionen wurden in vitro mit humanen gingivalen Fibroblasten (iHGFs) und osteoblastenähnlichen Saos-2-Zellen evaluiert. Das Verhalten von Weichgewebezellen wurde durch Live/Dead-Färbung, REM-Aufnahmen und Proliferationsassays bewertet, während die osteogene Differenzierung mittels alkalischer Phosphatase (ALP)-Aktivität und Alizarin-Rot-S-Färbung quantifiziert wurde. Die Ergebnisse zeigen, dass die Plasmabehandlung die Benetzbarkeit signifikant verbesserte (WCA-Reduktion von 75.72° auf nahe 0°), primär durch Sauerstofffunktionalitäten (C–O, C=O). Trotz zeitbedingter Hydrophilitätsabnahme infolge von Alterung blieb diese bei 15-minütiger Behandlung besser erhalten. Die Mikrohärte stieg zeitabhängig an. Oberflächenrauhigkeitsänderungen waren gering und statistisch insignifikant, jedoch zeigten längere Behandlungen tendenziell verstärktes Ätzen. Biologisch förderten plasmamodifizierte Oberflächen verbesserte Zelladhäsion, - ausbreitung und -proliferation. Bemerkenswerterweise wies die 4-minütige Behandlungsgruppe die günstigsten Ergebnisse bei ALP-Aktivität und Kalziumeinlagerung auf – sogar besser als die 15-minütige Gruppe. Dies deutet darauf hin, dass moderate Plasmaexposition eine optimale Oberflächenaktivierung erreicht, während negative Effekte übermäßiger Oxidation (z.B. Proteindenaturierung) vermieden werden. Die Befunde unterstreichen, dass Oberflächenchemie – nicht Rauheit – das Zellverhalten dominiert. Zusammenfassend verbessert die H₂/O₂-Niederdruckplasmabehandlung die Oberflächeneigenschaften und biologische Funktionalität von PEEK effektiv. Eine 4- minütige Behandlung bietet das optimale Gleichgewicht für positive Reaktionen von Weich- und Hartgewebezellen, was ihr klinisches Potenzial für dental- und orthopädische Implantate unterstreicht. Weitere Untersuchungen zu antimikrobiellen Eigenschaften, Gen-/Proteinexpressionsprofilen und in-vivo-Osseointegration sind jedoch erforderlich."]},{"key":"dc:format.extent","label":"Dc Format Extent","values":["viii, 68"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["free"]},{"key":"dc:title","label":"Title","values":["Enhancing the biocompatibility of PEEK implants through O2/H2 plasma treatment: Effects on surface properties and cell behavior"]},{"key":"dc:title.alternative","label":"Alternative Title","values":["Verbesserung der Biokompatibilität von PEEK-Implantaten durch O2/H2-Plasmabehandlung: Auswirkungen auf Oberflächeneigenschaften und Zellverhalten"]}]}],"canonical_facts":{"dc:contributor.committeemember":["N.N."],"dc:contributor.department":["Charité - Universitätsmedizin Berlin"],"dc:creator":["Weng, Shengxin"],"dc:date.issued":["2026"],"dc:description.abstract":["Polyetheretherketone (PEEK) has gained attention as a biomaterial in clinical applications due to its excellent mechanical properties, radiolucency, and chemical stability. However, its biologically inert surface limits direct integration with surrounding tissues, thereby constraining its broader clinical use. This study aimed to investigate the effects of low- pressure hydrogen–oxygen (H₂/O₂, 1:1) plasma surface modification on the physicochemical characteristics and biological performance of PEEK, to enhance both soft and hard tissue responses. A total of 276 PEEK specimens were fabricated and subjected to varying durations of H₂/O₂ low-pressure plasma treatment. Surface wettability, roughness, micro hardness, and chemical composition before and after treatment were assessed using water contact angle (WCA) measurements, optical profilometry, micro hardness testing, scanning electron microscopy (SEM), and X-ray photoelectron spectroscopy (XPS). The aging behavior of plasma-modified surfaces was monitored over 21 days. In vitro biological responses were evaluated using human gingival fibroblasts (iHGFs) and osteoblast-like Saos-2 cells. Soft tissue cell behavior was assessed via live/dead staining, SEM imaging, and proliferation assays, while osteogenic differentiation was evaluated through alkaline phosphatase (ALP) activity and Alizarin Red S staining. The results demonstrated that plasma treatment significantly enhanced surface wettability, reducing the WCA from 75.72° to nearly 0°, primarily due to the incorporation of oxygen-containing functional groups (C–O, C=O). Although surface hydrophilicity declined over time as a result of aging, it was better preserved in specimens treated for 15 minutes. Plasma treatment also led to a time-dependent increase in micro hardness. While surface roughness changes were minor and not statistically significant, longer treatment durations showed a trend toward increased surface etching. Biologically, plasma-modified surfaces promoted improved cell adhesion, spreading, and proliferation. Notably, the 4-minute treatment group exhibited the most favourable outcomes in terms of ALP activity and calcium deposition, surpassing even the 15-minute group. These results suggest that moderate plasma exposure can achieve optimal surface activation while avoiding the potential adverse effects of excessive oxidation, such as protein denaturation. The findings further emphasize that surface chemistry, rather than roughness, plays a dominant role in modulating cell behavior. In conclusion, H₂/O₂ low-pressure plasma treatment effectively enhances the surface properties and biological functionality of PEEK. A 4-minute treatment duration appears to offer the optimal balance for promoting favourable responses from both soft and hard tissue cells, highlighting its clinical potential in dental and orthopaedic implant applications. Nevertheless, further investigations are warranted to evaluate antimicrobial properties, gene and protein expression profiles, and in vivo osseointegration outcomes.","Polyetheretherketon (PEEK) hat als Biomaterial für klinische Anwendungen aufgrund seiner hervorragenden mechanischen Eigenschaften, Röntgentransparenz und chemischen Stabilität an Bedeutung gewonnen. Seine biologische Inertheit begrenzt jedoch die direkte Integration in umgebendes Gewebe, was den breiteren klinischen Einsatz einschränkt. Diese Studie untersuchte die Effekte einer Niederdruck-Wasserstoff- Sauerstoff-Plasmabehandlung (H₂/O₂, 1:1) auf die physikochemischen Eigenschaften und die biologische Performance von PEEK, um die Weich- und Hartgewebereaktionen zu verbessern. 276 PEEK-Proben wurden hergestellt und unterschiedlich langen H₂/O₂- Niederdruckplasmabehandlungen unterzogen. Oberflächenbenetzbarkeit, Rauheit, Mikrohärte und chemische Zusammensetzung vor/nach Behandlung wurden mittels Wasser-Kontaktwinkelmessungen (WCA), optischer Profilometrie, Mikrohärtetests, Rasterelektronenmikroskopie (REM) und Röntgenphotoelektronenspektroskopie (XPS) analysiert. Das Alterungsverhalten plasmamodifizierter Oberflächen wurde über 21 Tage beobachtet. Die biologischen Reaktionen wurden in vitro mit humanen gingivalen Fibroblasten (iHGFs) und osteoblastenähnlichen Saos-2-Zellen evaluiert. Das Verhalten von Weichgewebezellen wurde durch Live/Dead-Färbung, REM-Aufnahmen und Proliferationsassays bewertet, während die osteogene Differenzierung mittels alkalischer Phosphatase (ALP)-Aktivität und Alizarin-Rot-S-Färbung quantifiziert wurde. Die Ergebnisse zeigen, dass die Plasmabehandlung die Benetzbarkeit signifikant verbesserte (WCA-Reduktion von 75.72° auf nahe 0°), primär durch Sauerstofffunktionalitäten (C–O, C=O). Trotz zeitbedingter Hydrophilitätsabnahme infolge von Alterung blieb diese bei 15-minütiger Behandlung besser erhalten. Die Mikrohärte stieg zeitabhängig an. Oberflächenrauhigkeitsänderungen waren gering und statistisch insignifikant, jedoch zeigten längere Behandlungen tendenziell verstärktes Ätzen. Biologisch förderten plasmamodifizierte Oberflächen verbesserte Zelladhäsion, - ausbreitung und -proliferation. Bemerkenswerterweise wies die 4-minütige Behandlungsgruppe die günstigsten Ergebnisse bei ALP-Aktivität und Kalziumeinlagerung auf – sogar besser als die 15-minütige Gruppe. Dies deutet darauf hin, dass moderate Plasmaexposition eine optimale Oberflächenaktivierung erreicht, während negative Effekte übermäßiger Oxidation (z.B. Proteindenaturierung) vermieden werden. Die Befunde unterstreichen, dass Oberflächenchemie – nicht Rauheit – das Zellverhalten dominiert. Zusammenfassend verbessert die H₂/O₂-Niederdruckplasmabehandlung die Oberflächeneigenschaften und biologische Funktionalität von PEEK effektiv. Eine 4- minütige Behandlung bietet das optimale Gleichgewicht für positive Reaktionen von Weich- und Hartgewebezellen, was ihr klinisches Potenzial für dental- und orthopädische Implantate unterstreicht. Weitere Untersuchungen zu antimikrobiellen Eigenschaften, Gen-/Proteinexpressionsprofilen und in-vivo-Osseointegration sind jedoch erforderlich."],"dc:format.extent":["viii, 68"],"dc:identifier.uri":["https://refubium.fu-berlin.de/handle/fub188/51963","http://dx.doi.org/10.17169/refubium-51699"],"dc:identifier.urn":["urn:nbn:de:kobv:188-refubium-51963-9"],"dc:language":["eng"],"dc:rights.accessrights":["open access"],"dc:rights.proquest":["accept"],"dc:rights.uri":["https://www.fu-berlin.de/sites/ub/publizieren/refubium/rechtliches/index.html"],"dc:subject":["PEEK","Hydrogen/oxygen low-pressure plasma","Osteoconductive","Biocompatibility"],"dc:subject.ddc":["ddc:610"],"dcterms:accessrights":["free"],"dc:title":["Enhancing the biocompatibility of PEEK implants through O2/H2 plasma treatment: Effects on surface properties and cell behavior"],"dc:title.alternative":["Verbesserung der Biokompatibilität von PEEK-Implantaten durch O2/H2-Plasmabehandlung: Auswirkungen auf Oberflächeneigenschaften und Zellverhalten"],"dc:type":["doc-type:doctoralThesis"],"dc:type.dcmitype":["Text"],"person:gender":["female"]},"updated_at":"2026-11-19T03:53:47Z"}