{"id":{"repo_id":"gatech","oai_identifier":"oai:repository.gatech.edu:1853/10488"},"canonical_url":"https://search.ndltd.org/etd/gatech/oai:repository.gatech.edu:1853/10488","repository":{"repo_id":"gatech","name":"Georgia Tech","base_url":"https://repository.gatech.edu/server/oai/request"},"display":{"title":"Surface Modifications to Mitigate Refractory Degradation in High-Temperature Black Liquor Gasifiers","abstract":"Ceria (CeO2), chromia (Cr2O3), yttria-stabilized zirconia (Y2O3-ZrO2), and sodium cerium oxide (Na2CeO3) were used as barrier coatings on Ufala, an alumina-based ceramic refractory, to determine if they were effective at increasing the life of the refractory in a high-temperature black liquor gasification environment. The ceria, chromia, and yttria-stabilized zirconia coatings were applied at atmospheric pressure using a coating applicator at the Institute of Paper Science and Technology at the Georgia Institute of Technology. The sodium cerium oxide coatings in addition to the three other coating types were applied under atmospheric pressure at C3 International Technologies in Alpharetta, GA. The coated refractory, as well as a set of uncoated refractory used for baseline analysis, were tested using molten synthetic smelt at 1000C for 36 hours. Uncoated refractory samples were also tested for 12, 72, 120, and 168 hours in order to make a kinetic reaction rate determination. The refractory were analyzed using gravimetric and dimensional analysis, X-ray diffraction, scanning electron microscopy, and energy dispersive X-ray spectroscopy to determine the severity of the physical changes that occurred after exposure to molten smelt. The data gathered from these experiments were not able to conclude that barrier coatings are sufficient to impede corrosion of the Ufala refractory material in molten smelt.","abstract_html":"Ceria (CeO2), chromia (Cr2O3), yttria-stabilized zirconia (Y2O3-ZrO2), and sodium cerium oxide (Na2CeO3) were used as barrier coatings on Ufala, an alumina-based ceramic refractory, to determine if they were effective at increasing the life of the refractory in a high-temperature black liquor gasification environment. The ceria, chromia, and yttria-stabilized zirconia coatings were applied at atmospheric pressure using a coating applicator at the Institute of Paper Science and Technology at the Georgia Institute of Technology. The sodium cerium oxide coatings in addition to the three other coating types were applied under atmospheric pressure at C3 International Technologies in Alpharetta, GA. The coated refractory, as well as a set of uncoated refractory used for baseline analysis, were tested using molten synthetic smelt at 1000C for 36 hours. Uncoated refractory samples were also tested for 12, 72, 120, and 168 hours in order to make a kinetic reaction rate determination. The refractory were analyzed using gravimetric and dimensional analysis, X-ray diffraction, scanning electron microscopy, and energy dispersive X-ray spectroscopy to determine the severity of the physical changes that occurred after exposure to molten smelt. The data gathered from these experiments were not able to conclude that barrier coatings are sufficient to impede corrosion of the Ufala refractory material in molten smelt.","abstract_has_math":false,"creators":["Pallay, Krista Joy"],"institution":"Georgia Institute of Technology","degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":"Chemical Engineering","school":null,"contributors":[],"advisors":["Empie, Jeff","Singh, Preet M."],"committee_chairs":[],"committee_members":["Deng, Yulin"],"year":2006,"date_issued":"2006-04-03","date_published":"2006-04-03","updated_at":"2026-11-19T06:10:38Z","subjects":["Coating methods","Refractory materials","Metal oxide coatings","Metallic oxides","Coating processes"],"languages":["en_US"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://hdl.handle.net/1853/10488","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"http://hdl.handle.net/1853/10488","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","download_url":null,"download_label":null,"download_source":null,"access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://repository.gatech.edu/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Arepository.gatech.edu%3A1853%2F10488","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Empie, Jeff","Singh, Preet M."]},{"key":"dc:contributor.committeemember","label":"Committee Member","values":["Deng, Yulin"]},{"key":"dc:contributor.department","label":"Department","values":["Chemical Engineering"]},{"key":"dc:contributor.other","label":"Dc Contributor Other","values":["School of Chemical and Biomolecular Engineering","College of Engineering"]},{"key":"dc:creator","label":"Author","values":["Pallay, Krista Joy"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2006-06-09T18:11:49Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2006-06-09T18:11:49Z"]},{"key":"dc:date.issued","label":"Date","values":["2006-04-03"]},{"key":"dc:publisher","label":"Institution","values":["Georgia Institute of Technology"]},{"key":"dc:relation.advisorentity","label":"Dc Relation Advisorentity","values":["436052a4-5726-4887-bdbf-e726647a6d26"]},{"key":"dc:relation.ispartofseries","label":"Dc Relation Ispartofseries","values":["Master of Science in Chemical Engineering"]},{"key":"dc:relation.orgunit","label":"Dc Relation Orgunit","values":["6cfa2dc6-c5bf-4f6b-99a2-57105d8f7a6f","7c022d60-21d5-497c-b552-95e489a06569"]},{"key":"dc:relation.seriesentity","label":"Dc Relation Seriesentity","values":["18c50290-ac88-4cba-a523-b7a273d139bc"]},{"key":"dc:type","label":"Dc Type","values":["Text","Thesis"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Coating methods","Refractory materials","Metal oxide coatings"]},{"key":"dc:subject.lcsh","label":"Dc Subject Lcsh","values":["Refractory materials","Metallic oxides","Coating processes"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.iso","label":"Language (ISO)","values":["en_US"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["http://hdl.handle.net/1853/10488"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Ceria (CeO2), chromia (Cr2O3), yttria-stabilized zirconia (Y2O3-ZrO2), and sodium cerium oxide (Na2CeO3) were used as barrier coatings on Ufala, an alumina-based ceramic refractory, to determine if they were effective at increasing the life of the refractory in a high-temperature black liquor gasification environment. The ceria, chromia, and yttria-stabilized zirconia coatings were applied at atmospheric pressure using a coating applicator at the Institute of Paper Science and Technology at the Georgia Institute of Technology. The sodium cerium oxide coatings in addition to the three other coating types were applied under atmospheric pressure at C3 International Technologies in Alpharetta, GA. The coated refractory, as well as a set of uncoated refractory used for baseline analysis, were tested using molten synthetic smelt at 1000C for 36 hours. Uncoated refractory samples were also tested for 12, 72, 120, and 168 hours in order to make a kinetic reaction rate determination. The refractory were analyzed using gravimetric and dimensional analysis, X-ray diffraction, scanning electron microscopy, and energy dispersive X-ray spectroscopy to determine the severity of the physical changes that occurred after exposure to molten smelt. The data gathered from these experiments were not able to conclude that barrier coatings are sufficient to impede corrosion of the Ufala refractory material in molten smelt."]},{"key":"dc:description.degree","label":"Dc Description Degree","values":["M.S."]},{"key":"dc:format.extent","label":"Dc Format Extent","values":["9519246 bytes"]},{"key":"dc:format.mimetype","label":"Dc Format Mimetype","values":["application/pdf"]},{"key":"dc:title","label":"Title","values":["Surface Modifications to Mitigate Refractory Degradation in High-Temperature Black Liquor Gasifiers"]},{"key":"dspace:entity.type","label":"Dspace Entity Type","values":["Publication"]}]}],"canonical_facts":{"dc:contributor.advisor":["Empie, Jeff","Singh, Preet M."],"dc:contributor.committeemember":["Deng, Yulin"],"dc:contributor.department":["Chemical Engineering"],"dc:contributor.other":["School of Chemical and Biomolecular Engineering","College of Engineering"],"dc:creator":["Pallay, Krista Joy"],"dc:date.accessioned":["2006-06-09T18:11:49Z"],"dc:date.available":["2006-06-09T18:11:49Z"],"dc:date.issued":["2006-04-03"],"dc:description.abstract":["Ceria (CeO2), chromia (Cr2O3), yttria-stabilized zirconia (Y2O3-ZrO2), and sodium cerium oxide (Na2CeO3) were used as barrier coatings on Ufala, an alumina-based ceramic refractory, to determine if they were effective at increasing the life of the refractory in a high-temperature black liquor gasification environment. The ceria, chromia, and yttria-stabilized zirconia coatings were applied at atmospheric pressure using a coating applicator at the Institute of Paper Science and Technology at the Georgia Institute of Technology. The sodium cerium oxide coatings in addition to the three other coating types were applied under atmospheric pressure at C3 International Technologies in Alpharetta, GA. The coated refractory, as well as a set of uncoated refractory used for baseline analysis, were tested using molten synthetic smelt at 1000C for 36 hours. Uncoated refractory samples were also tested for 12, 72, 120, and 168 hours in order to make a kinetic reaction rate determination. The refractory were analyzed using gravimetric and dimensional analysis, X-ray diffraction, scanning electron microscopy, and energy dispersive X-ray spectroscopy to determine the severity of the physical changes that occurred after exposure to molten smelt. The data gathered from these experiments were not able to conclude that barrier coatings are sufficient to impede corrosion of the Ufala refractory material in molten smelt."],"dc:description.degree":["M.S."],"dc:format.extent":["9519246 bytes"],"dc:format.mimetype":["application/pdf"],"dc:identifier.uri":["http://hdl.handle.net/1853/10488"],"dc:language.iso":["en_US"],"dc:publisher":["Georgia Institute of Technology"],"dc:relation.advisorentity":["436052a4-5726-4887-bdbf-e726647a6d26"],"dc:relation.ispartofseries":["Master of Science in Chemical Engineering"],"dc:relation.orgunit":["6cfa2dc6-c5bf-4f6b-99a2-57105d8f7a6f","7c022d60-21d5-497c-b552-95e489a06569"],"dc:relation.seriesentity":["18c50290-ac88-4cba-a523-b7a273d139bc"],"dc:subject":["Coating methods","Refractory materials","Metal oxide coatings"],"dc:subject.lcsh":["Refractory materials","Metallic oxides","Coating processes"],"dc:title":["Surface Modifications to Mitigate Refractory Degradation in High-Temperature Black Liquor Gasifiers"],"dc:type":["Text","Thesis"],"dspace:entity.type":["Publication"]},"updated_at":"2026-11-19T06:10:38Z"}