{"id":{"repo_id":"gatech","oai_identifier":"oai:repository.gatech.edu:1853/7515"},"canonical_url":"https://search.ndltd.org/etd/gatech/oai:repository.gatech.edu:1853/7515","repository":{"repo_id":"gatech","name":"Georgia Tech","base_url":"https://repository.gatech.edu/server/oai/request"},"display":{"title":"Stress Intensity Solutions of Thermally Induced Cracks in a Combustor Liner Hot Spot Using Finite Element Analysis","abstract":"Thermally cycling a thin plate of nickel-based superalloy with an intense in-plane thermal gradient, or hot spot, produces thermally induced crack growth not represented by classic thermo-mechanical fatigue (TMF). With the max hot spot temperature at 1093 C (2000 F) of a 1.5 mm thick, 82.55 mm diameter circular plate of B-1900+Hf, annular buckling and bending stresses result during each thermal cycle which drive the crack initiation and propagation. A finite element analysis (FEA) model, using ANSYS 7.1, has been developed which models the buckling and as well as represents the stress intensity at simulated crack lengths upon cool down of each thermal cycle. The model approximates the out-of-plane response at heat-up within 5% error and a difference in the final displacement of 0.185 mm after twelve thermal cycles. Using published da/dN vs. Keff data, the number of cycles needed to grow the crack to the experimental arrest distance is modeled within 1 mm. The number of cycles to this point is within 5 out of 462 in comparison to the experimental test.","abstract_html":"Thermally cycling a thin plate of nickel-based superalloy with an intense in-plane thermal gradient, or hot spot, produces thermally induced crack growth not represented by classic thermo-mechanical fatigue (TMF). With the max hot spot temperature at 1093 C (2000 F) of a 1.5 mm thick, 82.55 mm diameter circular plate of B-1900+Hf, annular buckling and bending stresses result during each thermal cycle which drive the crack initiation and propagation. A finite element analysis (FEA) model, using ANSYS 7.1, has been developed which models the buckling and as well as represents the stress intensity at simulated crack lengths upon cool down of each thermal cycle. The model approximates the out-of-plane response at heat-up within 5% error and a difference in the final displacement of 0.185 mm after twelve thermal cycles. Using published da/dN vs. Keff data, the number of cycles needed to grow the crack to the experimental arrest distance is modeled within 1 mm. The number of cycles to this point is within 5 out of 462 in comparison to the experimental test.","abstract_has_math":false,"creators":["Rhymer, Donald William"],"institution":"Georgia Institute of Technology","degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":"Mechanical Engineering","school":null,"contributors":[],"advisors":["Johnson, W. Steven"],"committee_chairs":[],"committee_members":[],"year":2005,"date_issued":"2005-11-17","date_published":"2005-11-17","updated_at":"2026-11-19T06:07:03Z","subjects":["Fatigue crack growth","Geometric nonlinearity","Thermal gradient","Nickel alloys Cracking","Heat resistant alloys Thermal fatigue"],"languages":["en_US"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://hdl.handle.net/1853/7515","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"http://hdl.handle.net/1853/7515","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","download_url":null,"download_label":null,"download_source":null,"access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://repository.gatech.edu/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Arepository.gatech.edu%3A1853%2F7515","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Johnson, W. Steven"]},{"key":"dc:contributor.department","label":"Department","values":["Mechanical Engineering"]},{"key":"dc:contributor.other","label":"Dc Contributor Other","values":["George W. Woodruff School of Mechanical Engineering","College of Engineering"]},{"key":"dc:creator","label":"Author","values":["Rhymer, Donald William"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2006-01-18T22:18:28Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2006-01-18T22:18:28Z"]},{"key":"dc:date.issued","label":"Date","values":["2005-11-17"]},{"key":"dc:publisher","label":"Institution","values":["Georgia Institute of Technology"]},{"key":"dc:relation.advisorentity","label":"Dc Relation Advisorentity","values":["1f9c1a01-3dbf-497a-bead-e4f463f554bd"]},{"key":"dc:relation.orgunit","label":"Dc Relation Orgunit","values":["c01ff908-c25f-439b-bf10-a074ed886bb7","7c022d60-21d5-497c-b552-95e489a06569"]},{"key":"dc:type","label":"Dc Type","values":["Text","Dissertation"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Fatigue crack growth","Geometric nonlinearity","Thermal gradient"]},{"key":"dc:subject.lcsh","label":"Dc Subject Lcsh","values":["Nickel alloys Cracking","Heat resistant alloys Thermal fatigue"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.iso","label":"Language (ISO)","values":["en_US"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["http://hdl.handle.net/1853/7515"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Thermally cycling a thin plate of nickel-based superalloy with an intense in-plane thermal gradient, or hot spot, produces thermally induced crack growth not represented by classic thermo-mechanical fatigue (TMF). With the max hot spot temperature at 1093 C (2000 F) of a 1.5 mm thick, 82.55 mm diameter circular plate of B-1900+Hf, annular buckling and bending stresses result during each thermal cycle which drive the crack initiation and propagation. A finite element analysis (FEA) model, using ANSYS 7.1, has been developed which models the buckling and as well as represents the stress intensity at simulated crack lengths upon cool down of each thermal cycle. The model approximates the out-of-plane response at heat-up within 5% error and a difference in the final displacement of 0.185 mm after twelve thermal cycles. Using published da/dN vs. Keff data, the number of cycles needed to grow the crack to the experimental arrest distance is modeled within 1 mm. The number of cycles to this point is within 5 out of 462 in comparison to the experimental test."]},{"key":"dc:description.degree","label":"Dc Description Degree","values":["Ph.D."]},{"key":"dc:format.extent","label":"Dc Format Extent","values":["3952875 bytes"]},{"key":"dc:format.mimetype","label":"Dc Format Mimetype","values":["application/pdf"]},{"key":"dc:title","label":"Title","values":["Stress Intensity Solutions of Thermally Induced Cracks in a Combustor Liner Hot Spot Using Finite Element Analysis"]},{"key":"dspace:entity.type","label":"Dspace Entity Type","values":["Publication"]}]}],"canonical_facts":{"dc:contributor.advisor":["Johnson, W. Steven"],"dc:contributor.department":["Mechanical Engineering"],"dc:contributor.other":["George W. Woodruff School of Mechanical Engineering","College of Engineering"],"dc:creator":["Rhymer, Donald William"],"dc:date.accessioned":["2006-01-18T22:18:28Z"],"dc:date.available":["2006-01-18T22:18:28Z"],"dc:date.issued":["2005-11-17"],"dc:description.abstract":["Thermally cycling a thin plate of nickel-based superalloy with an intense in-plane thermal gradient, or hot spot, produces thermally induced crack growth not represented by classic thermo-mechanical fatigue (TMF). With the max hot spot temperature at 1093 C (2000 F) of a 1.5 mm thick, 82.55 mm diameter circular plate of B-1900+Hf, annular buckling and bending stresses result during each thermal cycle which drive the crack initiation and propagation. A finite element analysis (FEA) model, using ANSYS 7.1, has been developed which models the buckling and as well as represents the stress intensity at simulated crack lengths upon cool down of each thermal cycle. The model approximates the out-of-plane response at heat-up within 5% error and a difference in the final displacement of 0.185 mm after twelve thermal cycles. Using published da/dN vs. Keff data, the number of cycles needed to grow the crack to the experimental arrest distance is modeled within 1 mm. The number of cycles to this point is within 5 out of 462 in comparison to the experimental test."],"dc:description.degree":["Ph.D."],"dc:format.extent":["3952875 bytes"],"dc:format.mimetype":["application/pdf"],"dc:identifier.uri":["http://hdl.handle.net/1853/7515"],"dc:language.iso":["en_US"],"dc:publisher":["Georgia Institute of Technology"],"dc:relation.advisorentity":["1f9c1a01-3dbf-497a-bead-e4f463f554bd"],"dc:relation.orgunit":["c01ff908-c25f-439b-bf10-a074ed886bb7","7c022d60-21d5-497c-b552-95e489a06569"],"dc:subject":["Fatigue crack growth","Geometric nonlinearity","Thermal gradient"],"dc:subject.lcsh":["Nickel alloys Cracking","Heat resistant alloys Thermal fatigue"],"dc:title":["Stress Intensity Solutions of Thermally Induced Cracks in a Combustor Liner Hot Spot Using Finite Element Analysis"],"dc:type":["Text","Dissertation"],"dspace:entity.type":["Publication"]},"updated_at":"2026-11-19T06:07:03Z"}