{"id":{"repo_id":"mcmaster","oai_identifier":"oai:macsphere.mcmaster.ca:11375/13030"},"canonical_url":"https://search.ndltd.org/etd/mcmaster/oai:macsphere.mcmaster.ca:11375/13030","repository":{"repo_id":"mcmaster","name":"McMaster University","base_url":"https://macsphere.mcmaster.ca/server/oai/request"},"display":{"title":"A Study of the Mechanical Properties of Silicon-Based Thin Films Deposited by ECR-PECVD and ICP-CVD","abstract":"<p>Silicon-based dielectric thin films including amorphous hydrogenated aluminium-doped silicon oxides (<em>a-</em>SiAl<sub>x</sub>O<sub>y</sub>:H), amorphous hydrogenated silicon nitrides (<em>a-</em>SiN<sub>x</sub>:H), and amorphous hydrogenated silicon carbides (<em>a-</em>SiC<sub>x</sub>:H) were deposited by remote plasma chemical vapour deposition (RPECVD) techniques including electron cyclotron resonance plasma enhanced chemical vapour deposition (ECR-PECVD) and inductively-coupled-plasma chemical vapour deposition (ICP-CVD) on silicon (Si) wafers, soda-lime glass microscope slides, and glassy carbon (C) plates. Aluminium (Al) in the SiAlO films was incorporated by way of a metalorganic Al(TMHD)<sub>3</sub> precursor.</p> <p>Thickness, refractive index, and growth rate of the films were measured using variable angle spectroscopic ellipsometry (VASE). Film composition was measured using energy dispersive X-ray spectroscopy (EDX) for the SiAlO films and Rutherford backscattering spectrometry (RBS) for the SiC<sub>x</sub> films. Elastic modulus and hardness of the SiAlO and SiC<sub>x</sub> films were measured using nanoindentation and their adhesion was characterized via progressive load scratch testing.</p> <p>All films were observed to be optically transparent at near-IR and red wavelengths with many SiN<sub>x</sub> and SiC<sub>x</sub> films exhibiting significant optical absorption above 2.25eV. Modification of a previously developed deposition recipe produced doubled growth rates in SiN<sub>x</sub> and SiC<sub>x </sub>films. SiAlO films were produced with up to 1.6±0.1at% aluninium (Al) incorporation, while SiC<sub>x</sub> films with composition ranging from SiC<sub>0.25</sub>:H to SiC<sub>2</sub>:H could be produced depending on the growth gas flow ratios. SiAlO films exhibited hardness and reduced modulus (<em>H</em> and <em>E</em>) up to 8.2±0.4 and 75±2GPa, respectively; <em>H </em>and <em>E</em> for the SiC<sub>x </sub>filmsreached 11.9±0.2 and 87±3 GPa. Initially, adhesion to Si wafers was extremely poor with films delaminating at loads of 1.5±0.3N when scratched with a 3/16” alumina (Al<sub>2</sub>O<sub>3</sub>) sphere; implementation of a rigorous pre-deposition surface cleaning procedure produced films showing only cracking and no delamination up to 30N loads vs. a 200μm radius Rockwell C diamond stylus.</p>","abstract_html":"&lt;p&gt;Silicon-based dielectric thin films including amorphous hydrogenated aluminium-doped silicon oxides (&lt;em&gt;a-&lt;/em&gt;SiAl&lt;sub&gt;x&lt;/sub&gt;O&lt;sub&gt;y&lt;/sub&gt;:H), amorphous hydrogenated silicon nitrides (&lt;em&gt;a-&lt;/em&gt;SiN&lt;sub&gt;x&lt;/sub&gt;:H), and amorphous hydrogenated silicon carbides (&lt;em&gt;a-&lt;/em&gt;SiC&lt;sub&gt;x&lt;/sub&gt;:H) were deposited by remote plasma chemical vapour deposition (RPECVD) techniques including electron cyclotron resonance plasma enhanced chemical vapour deposition (ECR-PECVD) and inductively-coupled-plasma chemical vapour deposition (ICP-CVD) on silicon (Si) wafers, soda-lime glass microscope slides, and glassy carbon (C) plates. Aluminium (Al) in the SiAlO films was incorporated by way of a metalorganic Al(TMHD)&lt;sub&gt;3&lt;/sub&gt; precursor.&lt;/p&gt; &lt;p&gt;Thickness, refractive index, and growth rate of the films were measured using variable angle spectroscopic ellipsometry (VASE). Film composition was measured using energy dispersive X-ray spectroscopy (EDX) for the SiAlO films and Rutherford backscattering spectrometry (RBS) for the SiC&lt;sub&gt;x&lt;/sub&gt; films. Elastic modulus and hardness of the SiAlO and SiC&lt;sub&gt;x&lt;/sub&gt; films were measured using nanoindentation and their adhesion was characterized via progressive load scratch testing.&lt;/p&gt; &lt;p&gt;All films were observed to be optically transparent at near-IR and red wavelengths with many SiN&lt;sub&gt;x&lt;/sub&gt; and SiC&lt;sub&gt;x&lt;/sub&gt; films exhibiting significant optical absorption above 2.25eV. Modification of a previously developed deposition recipe produced doubled growth rates in SiN&lt;sub&gt;x&lt;/sub&gt; and SiC&lt;sub&gt;x &lt;/sub&gt;films. SiAlO films were produced with up to 1.6±0.1at% aluninium (Al) incorporation, while SiC&lt;sub&gt;x&lt;/sub&gt; films with composition ranging from SiC&lt;sub&gt;0.25&lt;/sub&gt;:H to SiC&lt;sub&gt;2&lt;/sub&gt;:H could be produced depending on the growth gas flow ratios. SiAlO films exhibited hardness and reduced modulus (&lt;em&gt;H&lt;/em&gt; and &lt;em&gt;E&lt;/em&gt;) up to 8.2±0.4 and 75±2GPa, respectively; &lt;em&gt;H &lt;/em&gt;and &lt;em&gt;E&lt;/em&gt; for the SiC&lt;sub&gt;x &lt;/sub&gt;filmsreached 11.9±0.2 and 87±3 GPa. Initially, adhesion to Si wafers was extremely poor with films delaminating at loads of 1.5±0.3N when scratched with a 3/16” alumina (Al&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;3&lt;/sub&gt;) sphere; implementation of a rigorous pre-deposition surface cleaning procedure produced films showing only cracking and no delamination up to 30N loads vs. a 200μm radius Rockwell C diamond stylus.&lt;/p&gt;","abstract_has_math":false,"creators":["Taggart, Owen"],"institution":null,"degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":"Engineering Physics","school":null,"contributors":[],"advisors":["Mascher, Peter","Turak, Ayse"],"committee_chairs":[],"committee_members":[],"year":2013,"date_issued":"2013-10","date_published":"2013-10","updated_at":"2026-11-18T19:30:39Z","subjects":["Silicon","Hardness","Modulus","Film","Nanoindentation","PECVD","Nanoscience and Nanotechnology"],"languages":[],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://doi.org/10.71548/8136"],"render_values":[{"text":"https://doi.org/10.71548/8136","href":"https://doi.org/10.71548/8136","code":true}]},{"key":"dc:identifier.other","label":"Dc Identifier Other","values":["opendissertations/7864","8909","4181913"],"render_values":[{"text":"opendissertations/7864","href":null,"code":true},{"text":"8909","href":null,"code":true},{"text":"4181913","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":"http://hdl.handle.net/11375/13030","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"http://hdl.handle.net/11375/13030","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","download_url":null,"download_label":null,"download_source":null,"access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://macsphere.mcmaster.ca/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Amacsphere.mcmaster.ca%3A11375%2F13030","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Mascher, Peter","Turak, Ayse"]},{"key":"dc:contributor.department","label":"Department","values":["Engineering Physics"]},{"key":"dc:creator","label":"Author","values":["Taggart, Owen"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2014-06-18T17:01:57Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2014-06-18T17:01:57Z"]},{"key":"dc:date.created","label":"Dc Date Created","values":["2013-05-29"]},{"key":"dc:date.issued","label":"Date","values":["2013-10"]},{"key":"dc:type","label":"Dc Type","values":["thesis"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Silicon","Hardness","Modulus","Film","Nanoindentation","PECVD","Nanoscience and Nanotechnology"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.other","label":"Dc Identifier Other","values":["opendissertations/7864","8909","4181913"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["http://hdl.handle.net/11375/13030","https://doi.org/10.71548/8136"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["<p>Silicon-based dielectric thin films including amorphous hydrogenated aluminium-doped silicon oxides (<em>a-</em>SiAl<sub>x</sub>O<sub>y</sub>:H), amorphous hydrogenated silicon nitrides (<em>a-</em>SiN<sub>x</sub>:H), and amorphous hydrogenated silicon carbides (<em>a-</em>SiC<sub>x</sub>:H) were deposited by remote plasma chemical vapour deposition (RPECVD) techniques including electron cyclotron resonance plasma enhanced chemical vapour deposition (ECR-PECVD) and inductively-coupled-plasma chemical vapour deposition (ICP-CVD) on silicon (Si) wafers, soda-lime glass microscope slides, and glassy carbon (C) plates. Aluminium (Al) in the SiAlO films was incorporated by way of a metalorganic Al(TMHD)<sub>3</sub> precursor.</p> <p>Thickness, refractive index, and growth rate of the films were measured using variable angle spectroscopic ellipsometry (VASE). Film composition was measured using energy dispersive X-ray spectroscopy (EDX) for the SiAlO films and Rutherford backscattering spectrometry (RBS) for the SiC<sub>x</sub> films. Elastic modulus and hardness of the SiAlO and SiC<sub>x</sub> films were measured using nanoindentation and their adhesion was characterized via progressive load scratch testing.</p> <p>All films were observed to be optically transparent at near-IR and red wavelengths with many SiN<sub>x</sub> and SiC<sub>x</sub> films exhibiting significant optical absorption above 2.25eV. Modification of a previously developed deposition recipe produced doubled growth rates in SiN<sub>x</sub> and SiC<sub>x </sub>films. SiAlO films were produced with up to 1.6±0.1at% aluninium (Al) incorporation, while SiC<sub>x</sub> films with composition ranging from SiC<sub>0.25</sub>:H to SiC<sub>2</sub>:H could be produced depending on the growth gas flow ratios. SiAlO films exhibited hardness and reduced modulus (<em>H</em> and <em>E</em>) up to 8.2±0.4 and 75±2GPa, respectively; <em>H </em>and <em>E</em> for the SiC<sub>x </sub>filmsreached 11.9±0.2 and 87±3 GPa. Initially, adhesion to Si wafers was extremely poor with films delaminating at loads of 1.5±0.3N when scratched with a 3/16” alumina (Al<sub>2</sub>O<sub>3</sub>) sphere; implementation of a rigorous pre-deposition surface cleaning procedure produced films showing only cracking and no delamination up to 30N loads vs. a 200μm radius Rockwell C diamond stylus.</p>"]},{"key":"dc:description.degree","label":"Dc Description Degree","values":["Master of Applied Science (MASc)"]},{"key":"dc:title","label":"Title","values":["A Study of the Mechanical Properties of Silicon-Based Thin Films Deposited by ECR-PECVD and ICP-CVD"]},{"key":"others:access_status","label":"Others Access Status","values":["open.access"]}]}],"canonical_facts":{"dc:contributor.advisor":["Mascher, Peter","Turak, Ayse"],"dc:contributor.department":["Engineering Physics"],"dc:creator":["Taggart, Owen"],"dc:date.accessioned":["2014-06-18T17:01:57Z"],"dc:date.available":["2014-06-18T17:01:57Z"],"dc:date.created":["2013-05-29"],"dc:date.issued":["2013-10"],"dc:description.abstract":["<p>Silicon-based dielectric thin films including amorphous hydrogenated aluminium-doped silicon oxides (<em>a-</em>SiAl<sub>x</sub>O<sub>y</sub>:H), amorphous hydrogenated silicon nitrides (<em>a-</em>SiN<sub>x</sub>:H), and amorphous hydrogenated silicon carbides (<em>a-</em>SiC<sub>x</sub>:H) were deposited by remote plasma chemical vapour deposition (RPECVD) techniques including electron cyclotron resonance plasma enhanced chemical vapour deposition (ECR-PECVD) and inductively-coupled-plasma chemical vapour deposition (ICP-CVD) on silicon (Si) wafers, soda-lime glass microscope slides, and glassy carbon (C) plates. Aluminium (Al) in the SiAlO films was incorporated by way of a metalorganic Al(TMHD)<sub>3</sub> precursor.</p> <p>Thickness, refractive index, and growth rate of the films were measured using variable angle spectroscopic ellipsometry (VASE). Film composition was measured using energy dispersive X-ray spectroscopy (EDX) for the SiAlO films and Rutherford backscattering spectrometry (RBS) for the SiC<sub>x</sub> films. Elastic modulus and hardness of the SiAlO and SiC<sub>x</sub> films were measured using nanoindentation and their adhesion was characterized via progressive load scratch testing.</p> <p>All films were observed to be optically transparent at near-IR and red wavelengths with many SiN<sub>x</sub> and SiC<sub>x</sub> films exhibiting significant optical absorption above 2.25eV. Modification of a previously developed deposition recipe produced doubled growth rates in SiN<sub>x</sub> and SiC<sub>x </sub>films. SiAlO films were produced with up to 1.6±0.1at% aluninium (Al) incorporation, while SiC<sub>x</sub> films with composition ranging from SiC<sub>0.25</sub>:H to SiC<sub>2</sub>:H could be produced depending on the growth gas flow ratios. SiAlO films exhibited hardness and reduced modulus (<em>H</em> and <em>E</em>) up to 8.2±0.4 and 75±2GPa, respectively; <em>H </em>and <em>E</em> for the SiC<sub>x </sub>filmsreached 11.9±0.2 and 87±3 GPa. Initially, adhesion to Si wafers was extremely poor with films delaminating at loads of 1.5±0.3N when scratched with a 3/16” alumina (Al<sub>2</sub>O<sub>3</sub>) sphere; implementation of a rigorous pre-deposition surface cleaning procedure produced films showing only cracking and no delamination up to 30N loads vs. a 200μm radius Rockwell C diamond stylus.</p>"],"dc:description.degree":["Master of Applied Science (MASc)"],"dc:identifier.other":["opendissertations/7864","8909","4181913"],"dc:identifier.uri":["http://hdl.handle.net/11375/13030","https://doi.org/10.71548/8136"],"dc:subject":["Silicon","Hardness","Modulus","Film","Nanoindentation","PECVD","Nanoscience and Nanotechnology"],"dc:title":["A Study of the Mechanical Properties of Silicon-Based Thin Films Deposited by ECR-PECVD and ICP-CVD"],"dc:type":["thesis"],"others:access_status":["open.access"]},"updated_at":"2026-11-18T19:30:39Z"}