{"id":{"repo_id":"nps","oai_identifier":"oai:calhoun.nps.edu:10945/25734"},"canonical_url":"https://search.ndltd.org/etd/nps/oai:calhoun.nps.edu:10945/25734","repository":{"repo_id":"nps","name":"Naval Postgraduate School","base_url":"https://calhoun.nps.edu/server/oai/request"},"display":{"title":"Characterization of the corrosion of a P-130x graphite fiber reinforced 6063 aluminum metal matrix composite.","abstract":"The corrosion behavior of a P-130x graphite fiber reinforced 6063 aluminum 0-90 cross plied metal matrix composite was studied. Electrochemical tests were performed on the composite and the monolithic matrix metal in aqueous 3.5% NaCl solutions. Immersion tests were performed on the composite in aqueous 3.5% NaCl solutions. The effects of pH, the presence of sulfite ions, and various heat treatments were investigated. The electrochemical tests included studies of galvanic corrosion, corrosion potential, galvanostaircase cyclic polarization and polarization resistance. Immersion tests showed accelerated corrosion at the exposed interfaces, with preferential attack at transverse fiber layers. Galvanic corrosion was large at low pH values, large graphite area fractions and when the matrix was in the over-aged state. The corrosion potential of the composite was found to be electronegative to the monolith when the Gr-Al interfaces were exposed to the electrolyte. Low pH values and over-aging increased pitting susceptibility. Solutionizing and quenching lowered pitting susceptibility at pH 8 but increased it at pH 4. Low pH values, the presence of sulfite ions and over- aging increased general corrosion rates.","abstract_html":"The corrosion behavior of a P-130x graphite fiber reinforced 6063 aluminum 0-90 cross plied metal matrix composite was studied. Electrochemical tests were performed on the composite and the monolithic matrix metal in aqueous 3.5% NaCl solutions. Immersion tests were performed on the composite in aqueous 3.5% NaCl solutions. The effects of pH, the presence of sulfite ions, and various heat treatments were investigated. The electrochemical tests included studies of galvanic corrosion, corrosion potential, galvanostaircase cyclic polarization and polarization resistance. Immersion tests showed accelerated corrosion at the exposed interfaces, with preferential attack at transverse fiber layers. Galvanic corrosion was large at low pH values, large graphite area fractions and when the matrix was in the over-aged state. The corrosion potential of the composite was found to be electronegative to the monolith when the Gr-Al interfaces were exposed to the electrolyte. Low pH values and over-aging increased pitting susceptibility. Solutionizing and quenching lowered pitting susceptibility at pH 8 but increased it at pH 4. Low pH values, the presence of sulfite ions and over- aging increased general corrosion rates.","abstract_has_math":false,"creators":["King, Joel David"],"institution":"Monterey, California. Naval Postgraduate School","degree_name":"M.S. in Mechanical Engineering","degree_level":"Masters","degree_discipline":"Mechanical Engineering","degree_department":"Mechanical Engineering","school":null,"contributors":[],"advisors":["Dutta, Indranath"],"committee_chairs":[],"committee_members":[],"year":1989,"date_issued":"1989-12","date_published":"1989-12","updated_at":"2026-11-21T22:39:08Z","subjects":[],"languages":[],"rights":["This publication is a work of the U.S. Government as defined in Title 17, United States Code, Section 101. Copyright protection is not available for this work in the United States.","Approved for public release; distribution is unlimited."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"https://hdl.handle.net/10945/25734","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"https://hdl.handle.net/10945/25734","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Anps%3Aoai%3Acalhoun.nps.edu%3A10945%2F25734","prefix":"oai_dc"},"source_record":{"url":"https://calhoun.nps.edu/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Acalhoun.nps.edu%3A10945%2F25734","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Dutta, Indranath"]},{"key":"dc:contributor.department","label":"Department","values":["Mechanical Engineering"]},{"key":"dc:contributor.other","label":"Dc Contributor Other","values":["Naval Postgraduate School (U.S.)"]},{"key":"dc:creator","label":"Author","values":["King, Joel David"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["December 1989"]},{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2013-01-23T21:53:40Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2013-01-23T21:53:40Z"]},{"key":"dc:date.issued","label":"Date","values":["1989-12"]},{"key":"dc:publisher","label":"Institution","values":["Monterey, California. Naval Postgraduate School"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Mechanical Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["Masters"]},{"key":"thesis:degree_name","label":"Degree Name","values":["M.S. in Mechanical Engineering"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["Naval Postgraduate School"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject.keyword","label":"Dc Subject Keyword","values":["aluminum","graphite","metal matrix composite","MMC","corrosion","electrochemical","sulfite","pH","heat treatment"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:rights","label":"Dc Rights","values":["This publication is a work of the U.S. Government as defined in Title 17, United States Code, Section 101. Copyright protection is not available for this work in the United States.","Approved for public release; distribution is unlimited."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://hdl.handle.net/10945/25734"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["The corrosion behavior of a P-130x graphite fiber reinforced 6063 aluminum 0-90 cross plied metal matrix composite was studied. Electrochemical tests were performed on the composite and the monolithic matrix metal in aqueous 3.5% NaCl solutions. Immersion tests were performed on the composite in aqueous 3.5% NaCl solutions. The effects of pH, the presence of sulfite ions, and various heat treatments were investigated. The electrochemical tests included studies of galvanic corrosion, corrosion potential, galvanostaircase cyclic polarization and polarization resistance. Immersion tests showed accelerated corrosion at the exposed interfaces, with preferential attack at transverse fiber layers. Galvanic corrosion was large at low pH values, large graphite area fractions and when the matrix was in the over-aged state. The corrosion potential of the composite was found to be electronegative to the monolith when the Gr-Al interfaces were exposed to the electrolyte. Low pH values and over-aging increased pitting susceptibility. Solutionizing and quenching lowered pitting susceptibility at pH 8 but increased it at pH 4. Low pH values, the presence of sulfite ions and over- aging increased general corrosion rates."]},{"key":"dc:description.uri","label":"Dc Description URI","values":["http://archive.org/details/characterization1094525734"]},{"key":"dc:format.extent","label":"Dc Format Extent","values":["83 p."]},{"key":"dc:title","label":"Title","values":["Characterization of the corrosion of a P-130x graphite fiber reinforced 6063 aluminum metal matrix composite."]},{"key":"dspace:entity.type","label":"Dspace Entity Type","values":["Publication"]},{"key":"local:contributor.affiliation","label":"Local Contributor Affiliation","values":["Lieutenant, United States Navy"]}]}],"canonical_facts":{"dc:contributor.advisor":["Dutta, Indranath"],"dc:contributor.department":["Mechanical Engineering"],"dc:contributor.other":["Naval Postgraduate School (U.S.)"],"dc:creator":["King, Joel David"],"dc:date":["December 1989"],"dc:date.accessioned":["2013-01-23T21:53:40Z"],"dc:date.available":["2013-01-23T21:53:40Z"],"dc:date.issued":["1989-12"],"dc:description.abstract":["The corrosion behavior of a P-130x graphite fiber reinforced 6063 aluminum 0-90 cross plied metal matrix composite was studied. Electrochemical tests were performed on the composite and the monolithic matrix metal in aqueous 3.5% NaCl solutions. Immersion tests were performed on the composite in aqueous 3.5% NaCl solutions. The effects of pH, the presence of sulfite ions, and various heat treatments were investigated. The electrochemical tests included studies of galvanic corrosion, corrosion potential, galvanostaircase cyclic polarization and polarization resistance. Immersion tests showed accelerated corrosion at the exposed interfaces, with preferential attack at transverse fiber layers. Galvanic corrosion was large at low pH values, large graphite area fractions and when the matrix was in the over-aged state. The corrosion potential of the composite was found to be electronegative to the monolith when the Gr-Al interfaces were exposed to the electrolyte. Low pH values and over-aging increased pitting susceptibility. Solutionizing and quenching lowered pitting susceptibility at pH 8 but increased it at pH 4. Low pH values, the presence of sulfite ions and over- aging increased general corrosion rates."],"dc:description.uri":["http://archive.org/details/characterization1094525734"],"dc:format.extent":["83 p."],"dc:identifier.uri":["https://hdl.handle.net/10945/25734"],"dc:publisher":["Monterey, California. Naval Postgraduate School"],"dc:rights":["This publication is a work of the U.S. Government as defined in Title 17, United States Code, Section 101. Copyright protection is not available for this work in the United States.","Approved for public release; distribution is unlimited."],"dc:subject.keyword":["aluminum","graphite","metal matrix composite","MMC","corrosion","electrochemical","sulfite","pH","heat treatment"],"dc:title":["Characterization of the corrosion of a P-130x graphite fiber reinforced 6063 aluminum metal matrix composite."],"dc:type":["Thesis"],"dspace:entity.type":["Publication"],"local:contributor.affiliation":["Lieutenant, United States Navy"],"thesis:degree_discipline":["Mechanical Engineering"],"thesis:degree_level":["Masters"],"thesis:degree_name":["M.S. in Mechanical Engineering"],"thesis:institution_name":["Naval Postgraduate School"]},"updated_at":"2026-11-21T22:39:08Z"}