{"id":{"repo_id":"ohiolink","oai_identifier":"oai:etd.ohiolink.edu:akron1444242002"},"canonical_url":"https://search.ndltd.org/etd/ohiolink/oai:etd.ohiolink.edu:akron1444242002","repository":{"repo_id":"ohiolink","name":"OhioLINK","base_url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai"},"display":{"title":"Extrinsic Influence of Environment on Tensile Response, Impact Toughness and Fracture Behavior of Four Metals: Ferrous Versus Non Ferrous","abstract":"In this thesis report an attempt is made to present and briefly discuss the specific influence of exposure, by way of immersion, to four different environments, pH+Salt, salt, pH and distilled water, for four chosen time period of one-week, two-weeks, three-weeks, and eight-weeks on the static (uni-axial tensile) and dynamic (impact) properties of two ferrous metals [i.e, 304L stainless steel, and alloy steel 4340 CF] and two non-ferrous metals [i.e., aluminum alloy 6061-T651 and aluminum alloy 7075]. Test specimens for both tensile tests and Charpy V-Notch impact tests on the as-provided material were precision machined and conformed to standards specified by the American Society for Testing Materials (ASTM). The pH and conductivity were measured using a pH meter and a conductivity meter. The pH and conductivity were measured in an attempt to establish the acidity-level or alkalinity-level of the chosen mediums. The impact toughness response and resultant fracture behavior of the four chosen metals, subsequent to their exposure, by way of immersion, for chosen time periods were studied over the temperatures range -180°C to +170°C. The tensile tests were performed in the room temperature (25oC), laboratory air (RH 55 pct.) environment. Final fracture behavior of the chosen metals was determined at both the macroscopic and fine microscopic levels. This was made possible following careful examination in a scanning electron microscope. After analyzing the data obtained it was observed that Salt medium was more corrosive among all the four environments and Distilled water was corrosion resistant medium. Steel was more corrosion resistant compared to Aluminum.","abstract_html":"In this thesis report an attempt is made to present and briefly discuss the specific influence of exposure, by way of immersion, to four different environments, pH+Salt, salt, pH and distilled water, for four chosen time period of one-week, two-weeks, three-weeks, and eight-weeks on the static (uni-axial tensile) and dynamic (impact) properties of two ferrous metals [i.e, 304L stainless steel, and alloy steel 4340 CF] and two non-ferrous metals [i.e., aluminum alloy 6061-T651 and aluminum alloy 7075]. Test specimens for both tensile tests and Charpy V-Notch impact tests on the as-provided material were precision machined and conformed to standards specified by the American Society for Testing Materials (ASTM). The pH and conductivity were measured using a pH meter and a conductivity meter. The pH and conductivity were measured in an attempt to establish the acidity-level or alkalinity-level of the chosen mediums. The impact toughness response and resultant fracture behavior of the four chosen metals, subsequent to their exposure, by way of immersion, for chosen time periods were studied over the temperatures range -180°C to +170°C. The tensile tests were performed in the room temperature (25oC), laboratory air (RH 55 pct.) environment. Final fracture behavior of the chosen metals was determined at both the macroscopic and fine microscopic levels. This was made possible following careful examination in a scanning electron microscope. After analyzing the data obtained it was observed that Salt medium was more corrosive among all the four environments and Distilled water was corrosion resistant medium. Steel was more corrosion resistant compared to Aluminum.","abstract_has_math":false,"creators":["Athasniya, Mohit"],"institution":"University of Akron","degree_name":"Master of Science in Engineering","degree_level":"masters","degree_discipline":"Civil Engineering","degree_department":null,"school":null,"contributors":[],"advisors":["Cutright, Teresa","Srivatsan, T.S"],"committee_chairs":[],"committee_members":[],"year":2015,"date_issued":"2015","date_published":"2015","updated_at":"2026-11-27T04:40:38Z","subjects":["Engineering","Corrosion, Stainless steel, Aluminum Alloys,"],"languages":["English"],"rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://rave.ohiolink.edu/etdc/view?acc_num=akron1444242002","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"http://rave.ohiolink.edu/etdc/view?acc_num=akron1444242002","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aohiolink%3Aoai%3Aetd.ohiolink.edu%3Aakron1444242002","prefix":"oai_dc"},"source_record":{"url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Aetd.ohiolink.edu%3Aakron1444242002","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Cutright, Teresa","Srivatsan, T.S"]},{"key":"dc:creator","label":"Author","values":["Athasniya, Mohit"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2015"]},{"key":"dc:publisher","label":"Institution","values":["University of Akron / OhioLINK"]},{"key":"dc:type","label":"Dc Type","values":["Electronic Thesis or Dissertation"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Civil Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["masters"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Master of Science in Engineering"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["University of Akron"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Engineering","Corrosion, Stainless steel, Aluminum Alloys,"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:rights","label":"Dc Rights","values":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://rave.ohiolink.edu/etdc/view?acc_num=akron1444242002"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["In this thesis report an attempt is made to present and briefly discuss the specific influence of exposure, by way of immersion, to four different environments, pH+Salt, salt, pH and distilled water, for four chosen time period of one-week, two-weeks, three-weeks, and eight-weeks on the static (uni-axial tensile) and dynamic (impact) properties of two ferrous metals [i.e, 304L stainless steel, and alloy steel 4340 CF] and two non-ferrous metals [i.e., aluminum alloy 6061-T651 and aluminum alloy 7075]. Test specimens for both tensile tests and Charpy V-Notch impact tests on the as-provided material were precision machined and conformed to standards specified by the American Society for Testing Materials (ASTM). The pH and conductivity were measured using a pH meter and a conductivity meter. The pH and conductivity were measured in an attempt to establish the acidity-level or alkalinity-level of the chosen mediums. The impact toughness response and resultant fracture behavior of the four chosen metals, subsequent to their exposure, by way of immersion, for chosen time periods were studied over the temperatures range -180°C to +170°C. The tensile tests were performed in the room temperature (25oC), laboratory air (RH 55 pct.) environment. Final fracture behavior of the chosen metals was determined at both the macroscopic and fine microscopic levels. This was made possible following careful examination in a scanning electron microscope. After analyzing the data obtained it was observed that Salt medium was more corrosive among all the four environments and Distilled water was corrosion resistant medium. Steel was more corrosion resistant compared to Aluminum."]},{"key":"dc:format","label":"Dc Format","values":["application/pdf","p.183","15.08 MB"]},{"key":"dc:title","label":"Title","values":["Extrinsic Influence of Environment on Tensile Response, Impact Toughness and Fracture Behavior of Four Metals: Ferrous Versus Non Ferrous"]}]}],"canonical_facts":{"dc:contributor.advisor":["Cutright, Teresa","Srivatsan, T.S"],"dc:creator":["Athasniya, Mohit"],"dc:date":["2015"],"dc:description":["In this thesis report an attempt is made to present and briefly discuss the specific influence of exposure, by way of immersion, to four different environments, pH+Salt, salt, pH and distilled water, for four chosen time period of one-week, two-weeks, three-weeks, and eight-weeks on the static (uni-axial tensile) and dynamic (impact) properties of two ferrous metals [i.e, 304L stainless steel, and alloy steel 4340 CF] and two non-ferrous metals [i.e., aluminum alloy 6061-T651 and aluminum alloy 7075]. Test specimens for both tensile tests and Charpy V-Notch impact tests on the as-provided material were precision machined and conformed to standards specified by the American Society for Testing Materials (ASTM). The pH and conductivity were measured using a pH meter and a conductivity meter. The pH and conductivity were measured in an attempt to establish the acidity-level or alkalinity-level of the chosen mediums. The impact toughness response and resultant fracture behavior of the four chosen metals, subsequent to their exposure, by way of immersion, for chosen time periods were studied over the temperatures range -180°C to +170°C. The tensile tests were performed in the room temperature (25oC), laboratory air (RH 55 pct.) environment. Final fracture behavior of the chosen metals was determined at both the macroscopic and fine microscopic levels. This was made possible following careful examination in a scanning electron microscope. After analyzing the data obtained it was observed that Salt medium was more corrosive among all the four environments and Distilled water was corrosion resistant medium. Steel was more corrosion resistant compared to Aluminum."],"dc:format":["application/pdf","p.183","15.08 MB"],"dc:identifier":["http://rave.ohiolink.edu/etdc/view?acc_num=akron1444242002"],"dc:language":["English"],"dc:publisher":["University of Akron / OhioLINK"],"dc:rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"dc:subject":["Engineering","Corrosion, Stainless steel, Aluminum Alloys,"],"dc:title":["Extrinsic Influence of Environment on Tensile Response, Impact Toughness and Fracture Behavior of Four Metals: Ferrous Versus Non Ferrous"],"dc:type":["Electronic Thesis or Dissertation"],"thesis:degree_discipline":["Civil Engineering"],"thesis:degree_level":["masters"],"thesis:degree_name":["Master of Science in Engineering"],"thesis:institution_name":["University of Akron"]},"updated_at":"2026-11-27T04:40:38Z"}