{"id":{"repo_id":"ohiolink","oai_identifier":"oai:etd.ohiolink.edu:akron1689205874590353"},"canonical_url":"https://search.ndltd.org/etd/ohiolink/oai:etd.ohiolink.edu:akron1689205874590353","repository":{"repo_id":"ohiolink","name":"OhioLINK","base_url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai"},"display":{"title":"Chain-level conceptual understanding of the deformation of semicrystalline polymers and the fracture of ductile glassy polymers","abstract":"Polymeric materials possess many useful properties, especially low density and high toughness. When crystallized, solvent resistance and temperature resistance are imparted. Predrawing can enhance their mechanical strength and toughness. However, whereas semicrystalline polymers (SCPs) like polyethylene (PE) and polypropylene (PP) are ductile, poly(lactic acid) (PLA) and poly (hydroxyalkanoates) (PHA) often show brittle behavior. In the face of a worldwide push for sustainable materials, it has become necessary to uncover the molecular picture that governs the processing-structure-property (P-S-P) relationships regarding the ductility (or lack thereof) of polymers. One example is how various types of predeformation can affect the mechanical properties. It has been shown [1] that pre-melt stretching of PLA in the near-affine limit close to the glass transition temperature Tg was shown to greatly enhance the strength and ductility of otherwise brittle PLA, and to produce a nanoconfined (NC) crystalline state whose length scale is on the order of the mesh size of the deformed chain network. Furthermore, this melt stretched PLA contained significant crystallinity and was transparent. In Chapter I, we show that after pre-melt shearing of amorphous PLA above Tg, the resultant crystalline and transparent PLA remains brittle. Both atomic force microscopy imaging (AFM) and small-angle x-ray scattering (SAXS) verify that melt-shearing has also produced an NC crystalline state. However, the brittle behavior of the melt-sheared PLA demonstrates the importance of having geometric condensation from processing. A similar NC crystalline state was generated in melt-sheared PET, thereby demonstrating the apparent universality of the methodology.In Chapter II, the P-S-P relationships are explored for SCPs that are crystallized under quiescent conditions. Since a disproportionate extent of effort has gone into researching the mechanisms of yielding rather than the origins of brittle failure or lack of drawability of SCPs, it is unclear how crystallization drives the material towards brittle or ductile failure and how tie-strands play a pivotal role in bringing about yielding and ductility. Much of this is also derived from uncertainty regarding how exactly crystallization has affected the initially entangled amorphous state and how the chain trajectory is affected [2]. In short, it is unclear from a first principles perspective how an SCP gains or loses ductility. Utilizing prior understanding regarding the drawability of glassy polymers [3], we attempt to construct a chain-level picture to begin to explain the processing-structure-property (P-S-P) relationships of SCPs, with emphasis on what makes SCPs drawable through variations of thermal history, drawing rate, and drawing temperature. We emphasize that ductility and drawability require a robust crystallization-reinforced chain network (CCN). Focusing our study to specimens subjected to uniaxial extension, we postulate that yielding occurs in the presence of sufficient pullout of load-bearing strands (such as tie strands) from the crystalline phase in order to cause partial melting of the crystalline phase. Subsequent drawability is then achieved provided sufficient load-bearing strands remain to keep the CCN intact through having sufficient number of surviving crystals and/or recrystallization to regenerate connectivity through the crystalline phase. Brittle failure by contrast is expected to involve an inability for the CCN to cause sufficient meltdown of the crystalline phase. From such observations we explore how the drawability and mechanical performance can be improved by predeformation in the crystalline or molten state.Another important topic in polymer science and engineering regards the premature failure of materials in the presence of a large crack or intentional cut. Two different approaches have emerged to try to understand the criterion for failure. Key to this debate is the uncertainty regarding the theoretical strength of polymers. Guided by prior understanding [3] regarding what we presume to be the inherent strength of isotropic amorphous polymer glasses, Chapter III conducts spatially-resolved birefringence measurements to quantify the stress intensification at a crack tip of ductile, glassy polyethylene terephthalate (PET) and polycarbonate (PC) films. From the measurements, we find that prior to yielding, a stress saturation zone (SSZ) of size rss ∼0.1 mm is observed in both polymers. More importantly, we find that the stress of the SSZ begins at a low stress value and grows monotonically with the applied load. At the onset of yielding near the crack tip, which was readily quantified by the residual birefringence observed in other cut specimens of PET and PC, the stress at the crack tip σtip was found to be similar or lower than the yield stress of the uncut specimen. Furthermore, σtip showed linear dependence with the mode I stress intensification constant KI. A characteristic length P from such linearity was found to be comparable to 2πrss, in which rss is conjectured to be related to the tip sharpness and the material characteristics. As such, the toughness of polymeric materials, given by the critical stress intensity factor KIc are both found to be dictated the magnitudes of P and the inherent strength of the material σinh, the latter expected to be equal to the stress at yielding or brittle failure in the uncut specimens [3].","abstract_html":"Polymeric materials possess many useful properties, especially low density and high toughness. When crystallized, solvent resistance and temperature resistance are imparted. Predrawing can enhance their mechanical strength and toughness. However, whereas semicrystalline polymers (SCPs) like polyethylene (PE) and polypropylene (PP) are ductile, poly(lactic acid) (PLA) and poly (hydroxyalkanoates) (PHA) often show brittle behavior. In the face of a worldwide push for sustainable materials, it has become necessary to uncover the molecular picture that governs the processing-structure-property (P-S-P) relationships regarding the ductility (or lack thereof) of polymers. One example is how various types of predeformation can affect the mechanical properties. It has been shown [1] that pre-melt stretching of PLA in the near-affine limit close to the glass transition temperature Tg was shown to greatly enhance the strength and ductility of otherwise brittle PLA, and to produce a nanoconfined (NC) crystalline state whose length scale is on the order of the mesh size of the deformed chain network. Furthermore, this melt stretched PLA contained significant crystallinity and was transparent. In Chapter I, we show that after pre-melt shearing of amorphous PLA above Tg, the resultant crystalline and transparent PLA remains brittle. Both atomic force microscopy imaging (AFM) and small-angle x-ray scattering (SAXS) verify that melt-shearing has also produced an NC crystalline state. However, the brittle behavior of the melt-sheared PLA demonstrates the importance of having geometric condensation from processing. A similar NC crystalline state was generated in melt-sheared PET, thereby demonstrating the apparent universality of the methodology.In Chapter II, the P-S-P relationships are explored for SCPs that are crystallized under quiescent conditions. Since a disproportionate extent of effort has gone into researching the mechanisms of yielding rather than the origins of brittle failure or lack of drawability of SCPs, it is unclear how crystallization drives the material towards brittle or ductile failure and how tie-strands play a pivotal role in bringing about yielding and ductility. Much of this is also derived from uncertainty regarding how exactly crystallization has affected the initially entangled amorphous state and how the chain trajectory is affected [2]. In short, it is unclear from a first principles perspective how an SCP gains or loses ductility. Utilizing prior understanding regarding the drawability of glassy polymers [3], we attempt to construct a chain-level picture to begin to explain the processing-structure-property (P-S-P) relationships of SCPs, with emphasis on what makes SCPs drawable through variations of thermal history, drawing rate, and drawing temperature. We emphasize that ductility and drawability require a robust crystallization-reinforced chain network (CCN). Focusing our study to specimens subjected to uniaxial extension, we postulate that yielding occurs in the presence of sufficient pullout of load-bearing strands (such as tie strands) from the crystalline phase in order to cause partial melting of the crystalline phase. Subsequent drawability is then achieved provided sufficient load-bearing strands remain to keep the CCN intact through having sufficient number of surviving crystals and/or recrystallization to regenerate connectivity through the crystalline phase. Brittle failure by contrast is expected to involve an inability for the CCN to cause sufficient meltdown of the crystalline phase. From such observations we explore how the drawability and mechanical performance can be improved by predeformation in the crystalline or molten state.Another important topic in polymer science and engineering regards the premature failure of materials in the presence of a large crack or intentional cut. Two different approaches have emerged to try to understand the criterion for failure. Key to this debate is the uncertainty regarding the theoretical strength of polymers. Guided by prior understanding [3] regarding what we presume to be the inherent strength of isotropic amorphous polymer glasses, Chapter III conducts spatially-resolved birefringence measurements to quantify the stress intensification at a crack tip of ductile, glassy polyethylene terephthalate (PET) and polycarbonate (PC) films. From the measurements, we find that prior to yielding, a stress saturation zone (SSZ) of size rss ∼0.1 mm is observed in both polymers. More importantly, we find that the stress of the SSZ begins at a low stress value and grows monotonically with the applied load. At the onset of yielding near the crack tip, which was readily quantified by the residual birefringence observed in other cut specimens of PET and PC, the stress at the crack tip σtip was found to be similar or lower than the yield stress of the uncut specimen. Furthermore, σtip showed linear dependence with the mode I stress intensification constant KI. A characteristic length P from such linearity was found to be comparable to 2πrss, in which rss is conjectured to be related to the tip sharpness and the material characteristics. As such, the toughness of polymeric materials, given by the critical stress intensity factor KIc are both found to be dictated the magnitudes of P and the inherent strength of the material σinh, the latter expected to be equal to the stress at yielding or brittle failure in the uncut specimens [3].","abstract_has_math":false,"creators":["Smith, Travis"],"institution":"University of Akron","degree_name":"Doctor of Philosophy","degree_level":"doctoral","degree_discipline":"Polymer Science","degree_department":null,"school":null,"contributors":[],"advisors":["Wang, Shi-Qing"],"committee_chairs":["Eagan, James"],"committee_members":[],"year":2023,"date_issued":"2023-08-02","date_published":"2023-08-02","updated_at":"2026-11-27T04:58:57Z","subjects":["Plastics","Physics","ductility, melt-shear deformation, nanoconfined crystallization, processing-structure-property relationship, semicrystalline polymers, fracture mechanics, inherent strength, plastics, birefringence, intrinsic flaws"],"languages":["English"],"rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://rave.ohiolink.edu/etdc/view?acc_num=akron1689205874590353","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"http://rave.ohiolink.edu/etdc/view?acc_num=akron1689205874590353","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aohiolink%3Aoai%3Aetd.ohiolink.edu%3Aakron1689205874590353","prefix":"oai_dc"},"source_record":{"url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Aetd.ohiolink.edu%3Aakron1689205874590353","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Wang, Shi-Qing"]},{"key":"dc:contributor.committeechair","label":"Committee Chair","values":["Eagan, James"]},{"key":"dc:creator","label":"Author","values":["Smith, Travis"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2023-08-02"]},{"key":"dc:publisher","label":"Institution","values":["University of Akron / OhioLINK"]},{"key":"dc:type","label":"Dc Type","values":["Electronic Thesis or Dissertation"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Polymer Science"]},{"key":"thesis:degree_level","label":"Degree Level","values":["doctoral"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Doctor of Philosophy"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["University of Akron"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Plastics","Physics","ductility, melt-shear deformation, nanoconfined crystallization, processing-structure-property relationship, semicrystalline polymers, fracture mechanics, inherent strength, plastics, birefringence, intrinsic flaws"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:rights","label":"Dc Rights","values":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://rave.ohiolink.edu/etdc/view?acc_num=akron1689205874590353"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["Polymeric materials possess many useful properties, especially low density and high toughness. When crystallized, solvent resistance and temperature resistance are imparted. Predrawing can enhance their mechanical strength and toughness. However, whereas semicrystalline polymers (SCPs) like polyethylene (PE) and polypropylene (PP) are ductile, poly(lactic acid) (PLA) and poly (hydroxyalkanoates) (PHA) often show brittle behavior. In the face of a worldwide push for sustainable materials, it has become necessary to uncover the molecular picture that governs the processing-structure-property (P-S-P) relationships regarding the ductility (or lack thereof) of polymers. One example is how various types of predeformation can affect the mechanical properties. It has been shown [1] that pre-melt stretching of PLA in the near-affine limit close to the glass transition temperature Tg was shown to greatly enhance the strength and ductility of otherwise brittle PLA, and to produce a nanoconfined (NC) crystalline state whose length scale is on the order of the mesh size of the deformed chain network. Furthermore, this melt stretched PLA contained significant crystallinity and was transparent. In Chapter I, we show that after pre-melt shearing of amorphous PLA above Tg, the resultant crystalline and transparent PLA remains brittle. Both atomic force microscopy imaging (AFM) and small-angle x-ray scattering (SAXS) verify that melt-shearing has also produced an NC crystalline state. However, the brittle behavior of the melt-sheared PLA demonstrates the importance of having geometric condensation from processing. A similar NC crystalline state was generated in melt-sheared PET, thereby demonstrating the apparent universality of the methodology.In Chapter II, the P-S-P relationships are explored for SCPs that are crystallized under quiescent conditions. Since a disproportionate extent of effort has gone into researching the mechanisms of yielding rather than the origins of brittle failure or lack of drawability of SCPs, it is unclear how crystallization drives the material towards brittle or ductile failure and how tie-strands play a pivotal role in bringing about yielding and ductility. Much of this is also derived from uncertainty regarding how exactly crystallization has affected the initially entangled amorphous state and how the chain trajectory is affected [2]. In short, it is unclear from a first principles perspective how an SCP gains or loses ductility. Utilizing prior understanding regarding the drawability of glassy polymers [3], we attempt to construct a chain-level picture to begin to explain the processing-structure-property (P-S-P) relationships of SCPs, with emphasis on what makes SCPs drawable through variations of thermal history, drawing rate, and drawing temperature. We emphasize that ductility and drawability require a robust crystallization-reinforced chain network (CCN). Focusing our study to specimens subjected to uniaxial extension, we postulate that yielding occurs in the presence of sufficient pullout of load-bearing strands (such as tie strands) from the crystalline phase in order to cause partial melting of the crystalline phase. Subsequent drawability is then achieved provided sufficient load-bearing strands remain to keep the CCN intact through having sufficient number of surviving crystals and/or recrystallization to regenerate connectivity through the crystalline phase. Brittle failure by contrast is expected to involve an inability for the CCN to cause sufficient meltdown of the crystalline phase. From such observations we explore how the drawability and mechanical performance can be improved by predeformation in the crystalline or molten state.Another important topic in polymer science and engineering regards the premature failure of materials in the presence of a large crack or intentional cut. Two different approaches have emerged to try to understand the criterion for failure. Key to this debate is the uncertainty regarding the theoretical strength of polymers. Guided by prior understanding [3] regarding what we presume to be the inherent strength of isotropic amorphous polymer glasses, Chapter III conducts spatially-resolved birefringence measurements to quantify the stress intensification at a crack tip of ductile, glassy polyethylene terephthalate (PET) and polycarbonate (PC) films. From the measurements, we find that prior to yielding, a stress saturation zone (SSZ) of size rss ∼0.1 mm is observed in both polymers. More importantly, we find that the stress of the SSZ begins at a low stress value and grows monotonically with the applied load. At the onset of yielding near the crack tip, which was readily quantified by the residual birefringence observed in other cut specimens of PET and PC, the stress at the crack tip σtip was found to be similar or lower than the yield stress of the uncut specimen. Furthermore, σtip showed linear dependence with the mode I stress intensification constant KI. A characteristic length P from such linearity was found to be comparable to 2πrss, in which rss is conjectured to be related to the tip sharpness and the material characteristics. As such, the toughness of polymeric materials, given by the critical stress intensity factor KIc are both found to be dictated the magnitudes of P and the inherent strength of the material σinh, the latter expected to be equal to the stress at yielding or brittle failure in the uncut specimens [3]."]},{"key":"dc:format","label":"Dc Format","values":["application/pdf","p.167","41.54 MB"]},{"key":"dc:title","label":"Title","values":["Chain-level conceptual understanding of the deformation of semicrystalline polymers and the fracture of ductile glassy polymers"]}]}],"canonical_facts":{"dc:contributor.advisor":["Wang, Shi-Qing"],"dc:contributor.committeechair":["Eagan, James"],"dc:creator":["Smith, Travis"],"dc:date":["2023-08-02"],"dc:description":["Polymeric materials possess many useful properties, especially low density and high toughness. When crystallized, solvent resistance and temperature resistance are imparted. Predrawing can enhance their mechanical strength and toughness. However, whereas semicrystalline polymers (SCPs) like polyethylene (PE) and polypropylene (PP) are ductile, poly(lactic acid) (PLA) and poly (hydroxyalkanoates) (PHA) often show brittle behavior. In the face of a worldwide push for sustainable materials, it has become necessary to uncover the molecular picture that governs the processing-structure-property (P-S-P) relationships regarding the ductility (or lack thereof) of polymers. One example is how various types of predeformation can affect the mechanical properties. It has been shown [1] that pre-melt stretching of PLA in the near-affine limit close to the glass transition temperature Tg was shown to greatly enhance the strength and ductility of otherwise brittle PLA, and to produce a nanoconfined (NC) crystalline state whose length scale is on the order of the mesh size of the deformed chain network. Furthermore, this melt stretched PLA contained significant crystallinity and was transparent. In Chapter I, we show that after pre-melt shearing of amorphous PLA above Tg, the resultant crystalline and transparent PLA remains brittle. Both atomic force microscopy imaging (AFM) and small-angle x-ray scattering (SAXS) verify that melt-shearing has also produced an NC crystalline state. However, the brittle behavior of the melt-sheared PLA demonstrates the importance of having geometric condensation from processing. A similar NC crystalline state was generated in melt-sheared PET, thereby demonstrating the apparent universality of the methodology.In Chapter II, the P-S-P relationships are explored for SCPs that are crystallized under quiescent conditions. Since a disproportionate extent of effort has gone into researching the mechanisms of yielding rather than the origins of brittle failure or lack of drawability of SCPs, it is unclear how crystallization drives the material towards brittle or ductile failure and how tie-strands play a pivotal role in bringing about yielding and ductility. Much of this is also derived from uncertainty regarding how exactly crystallization has affected the initially entangled amorphous state and how the chain trajectory is affected [2]. In short, it is unclear from a first principles perspective how an SCP gains or loses ductility. Utilizing prior understanding regarding the drawability of glassy polymers [3], we attempt to construct a chain-level picture to begin to explain the processing-structure-property (P-S-P) relationships of SCPs, with emphasis on what makes SCPs drawable through variations of thermal history, drawing rate, and drawing temperature. We emphasize that ductility and drawability require a robust crystallization-reinforced chain network (CCN). Focusing our study to specimens subjected to uniaxial extension, we postulate that yielding occurs in the presence of sufficient pullout of load-bearing strands (such as tie strands) from the crystalline phase in order to cause partial melting of the crystalline phase. Subsequent drawability is then achieved provided sufficient load-bearing strands remain to keep the CCN intact through having sufficient number of surviving crystals and/or recrystallization to regenerate connectivity through the crystalline phase. Brittle failure by contrast is expected to involve an inability for the CCN to cause sufficient meltdown of the crystalline phase. From such observations we explore how the drawability and mechanical performance can be improved by predeformation in the crystalline or molten state.Another important topic in polymer science and engineering regards the premature failure of materials in the presence of a large crack or intentional cut. Two different approaches have emerged to try to understand the criterion for failure. Key to this debate is the uncertainty regarding the theoretical strength of polymers. Guided by prior understanding [3] regarding what we presume to be the inherent strength of isotropic amorphous polymer glasses, Chapter III conducts spatially-resolved birefringence measurements to quantify the stress intensification at a crack tip of ductile, glassy polyethylene terephthalate (PET) and polycarbonate (PC) films. From the measurements, we find that prior to yielding, a stress saturation zone (SSZ) of size rss ∼0.1 mm is observed in both polymers. More importantly, we find that the stress of the SSZ begins at a low stress value and grows monotonically with the applied load. At the onset of yielding near the crack tip, which was readily quantified by the residual birefringence observed in other cut specimens of PET and PC, the stress at the crack tip σtip was found to be similar or lower than the yield stress of the uncut specimen. Furthermore, σtip showed linear dependence with the mode I stress intensification constant KI. A characteristic length P from such linearity was found to be comparable to 2πrss, in which rss is conjectured to be related to the tip sharpness and the material characteristics. As such, the toughness of polymeric materials, given by the critical stress intensity factor KIc are both found to be dictated the magnitudes of P and the inherent strength of the material σinh, the latter expected to be equal to the stress at yielding or brittle failure in the uncut specimens [3]."],"dc:format":["application/pdf","p.167","41.54 MB"],"dc:identifier":["http://rave.ohiolink.edu/etdc/view?acc_num=akron1689205874590353"],"dc:language":["English"],"dc:publisher":["University of Akron / OhioLINK"],"dc:rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"dc:subject":["Plastics","Physics","ductility, melt-shear deformation, nanoconfined crystallization, processing-structure-property relationship, semicrystalline polymers, fracture mechanics, inherent strength, plastics, birefringence, intrinsic flaws"],"dc:title":["Chain-level conceptual understanding of the deformation of semicrystalline polymers and the fracture of ductile glassy polymers"],"dc:type":["Electronic Thesis or Dissertation"],"thesis:degree_discipline":["Polymer Science"],"thesis:degree_level":["doctoral"],"thesis:degree_name":["Doctor of Philosophy"],"thesis:institution_name":["University of Akron"]},"updated_at":"2026-11-27T04:58:57Z"}