{"id":{"repo_id":"ohiolink","oai_identifier":"oai:etd.ohiolink.edu:case1297369701"},"canonical_url":"https://search.ndltd.org/etd/ohiolink/oai:etd.ohiolink.edu:case1297369701","repository":{"repo_id":"ohiolink","name":"OhioLINK","base_url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai"},"display":{"title":"EFFECT OF LOW TEMPERATURE CARBURIZATION ON THE MECHANICAL BEHAVIOR OF GASEOUS HYDROGEN-CHARGED 316L STAINLESS STEEL","abstract":"<p>The mechanical behavior of hydrogen-charged 316L stainless steel has been studied in samples containing sharp fatigue-induced pre-cracks, and compared with material that had been carburized at low temperatures following pre-cracking. The hydrogen charging involved exposure to high pressure (~138 MPa) H2 at 573 K for 24 days.</p><p>Non-treated samples either stayed elastic in low stress intensity range or exhibited plasticity at the crack tip at high range; no hydrogen-induced cracking could be observed. On the carburized sample, however, the main crack extended during loading. The variation of crack depth along the crack was verified and reveals that the crack becomes shallower as it approached the newly extended crack tip. The threshold stress intensity factor for the hardened case, Kth, is calculated based on this observation. Plastic zone evolution at the crack tip suggests the presence of hydrogen facilitates the motion of dislocations at the room temperature.</p>","abstract_html":"&lt;p&gt;The mechanical behavior of hydrogen-charged 316L stainless steel has been studied in samples containing sharp fatigue-induced pre-cracks, and compared with material that had been carburized at low temperatures following pre-cracking. The hydrogen charging involved exposure to high pressure (~138 MPa) H2 at 573 K for 24 days.&lt;/p&gt;&lt;p&gt;Non-treated samples either stayed elastic in low stress intensity range or exhibited plasticity at the crack tip at high range; no hydrogen-induced cracking could be observed. On the carburized sample, however, the main crack extended during loading. The variation of crack depth along the crack was verified and reveals that the crack becomes shallower as it approached the newly extended crack tip. The threshold stress intensity factor for the hardened case, Kth, is calculated based on this observation. Plastic zone evolution at the crack tip suggests the presence of hydrogen facilitates the motion of dislocations at the room temperature.&lt;/p&gt;","abstract_has_math":false,"creators":["Wang, Danqi"],"institution":"Case Western Reserve University School of Graduate Studies","degree_name":"Master of Engineering","degree_level":"masters","degree_discipline":"Materials Science and Engineering","degree_department":null,"school":null,"contributors":["Heuer, Arthur"],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2011,"date_issued":"2011-05-04","date_published":"2011-05-04","updated_at":"2026-11-26T03:18:31Z","subjects":["Materials Science","low temperature carburization","austenitic stainless steel","hydrogen-induced cracking"],"languages":["English"],"rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://rave.ohiolink.edu/etdc/view?acc_num=case1297369701","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"http://rave.ohiolink.edu/etdc/view?acc_num=case1297369701","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aohiolink%3Aoai%3Aetd.ohiolink.edu%3Acase1297369701","prefix":"oai_dc"},"source_record":{"url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Aetd.ohiolink.edu%3Acase1297369701","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor","label":"Contributor","values":["Heuer, Arthur"]},{"key":"dc:creator","label":"Author","values":["Wang, Danqi"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2011-05-04"]},{"key":"dc:publisher","label":"Institution","values":["Case Western Reserve University School of Graduate Studies / OhioLINK"]},{"key":"dc:type","label":"Dc Type","values":["Electronic Thesis or Dissertation"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Materials Science and Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["masters"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Master of Engineering"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["Case Western Reserve University School of Graduate Studies"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Materials Science","low temperature carburization","austenitic stainless steel","hydrogen-induced cracking"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:rights","label":"Dc Rights","values":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://rave.ohiolink.edu/etdc/view?acc_num=case1297369701"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["<p>The mechanical behavior of hydrogen-charged 316L stainless steel has been studied in samples containing sharp fatigue-induced pre-cracks, and compared with material that had been carburized at low temperatures following pre-cracking. The hydrogen charging involved exposure to high pressure (~138 MPa) H2 at 573 K for 24 days.</p><p>Non-treated samples either stayed elastic in low stress intensity range or exhibited plasticity at the crack tip at high range; no hydrogen-induced cracking could be observed. On the carburized sample, however, the main crack extended during loading. The variation of crack depth along the crack was verified and reveals that the crack becomes shallower as it approached the newly extended crack tip. The threshold stress intensity factor for the hardened case, Kth, is calculated based on this observation. Plastic zone evolution at the crack tip suggests the presence of hydrogen facilitates the motion of dislocations at the room temperature.</p>"]},{"key":"dc:format","label":"Dc Format","values":["application/pdf","8.26 MB"]},{"key":"dc:title","label":"Title","values":["EFFECT OF LOW TEMPERATURE CARBURIZATION ON THE MECHANICAL BEHAVIOR OF GASEOUS HYDROGEN-CHARGED 316L STAINLESS STEEL"]}]}],"canonical_facts":{"dc:contributor":["Heuer, Arthur"],"dc:creator":["Wang, Danqi"],"dc:date":["2011-05-04"],"dc:description":["<p>The mechanical behavior of hydrogen-charged 316L stainless steel has been studied in samples containing sharp fatigue-induced pre-cracks, and compared with material that had been carburized at low temperatures following pre-cracking. The hydrogen charging involved exposure to high pressure (~138 MPa) H2 at 573 K for 24 days.</p><p>Non-treated samples either stayed elastic in low stress intensity range or exhibited plasticity at the crack tip at high range; no hydrogen-induced cracking could be observed. On the carburized sample, however, the main crack extended during loading. The variation of crack depth along the crack was verified and reveals that the crack becomes shallower as it approached the newly extended crack tip. The threshold stress intensity factor for the hardened case, Kth, is calculated based on this observation. Plastic zone evolution at the crack tip suggests the presence of hydrogen facilitates the motion of dislocations at the room temperature.</p>"],"dc:format":["application/pdf","8.26 MB"],"dc:identifier":["http://rave.ohiolink.edu/etdc/view?acc_num=case1297369701"],"dc:language":["English"],"dc:publisher":["Case Western Reserve University School of Graduate Studies / OhioLINK"],"dc:rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"dc:subject":["Materials Science","low temperature carburization","austenitic stainless steel","hydrogen-induced cracking"],"dc:title":["EFFECT OF LOW TEMPERATURE CARBURIZATION ON THE MECHANICAL BEHAVIOR OF GASEOUS HYDROGEN-CHARGED 316L STAINLESS STEEL"],"dc:type":["Electronic Thesis or Dissertation"],"thesis:degree_discipline":["Materials Science and Engineering"],"thesis:degree_level":["masters"],"thesis:degree_name":["Master of Engineering"],"thesis:institution_name":["Case Western Reserve University School of Graduate Studies"]},"updated_at":"2026-11-26T03:18:31Z"}