{"id":{"repo_id":"ohiolink","oai_identifier":"oai:etd.ohiolink.edu:case1307733545"},"canonical_url":"https://search.ndltd.org/etd/ohiolink/oai:etd.ohiolink.edu:case1307733545","repository":{"repo_id":"ohiolink","name":"OhioLINK","base_url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai"},"display":{"title":"The Dissolution of Iron from Automotive Steel Sheets in a Molten Zinc Bath and the Kinetics of the Nucleation and Growth of Dross Particles","abstract":"Hot-dip galvanizing (HDG) is a well-known process that increases the resistance of a steel strip to corrosion. Immersion of an automotive steel sheet in a galvanizing bath initiates a dissolution reaction. The flux of iron from the steel surface into the liquid zinc bath provides a driving force for the formation of an inhibition layer and the precipitation of dross particles. Such reactions involve the kinetics of nucleation and growth of intermetallic phases. This study addresses two main issues. First, the iron dissolution rate constant is governed by the solubility of iron in the liquid zinc under a metastable state between the pure bcc iron and the liquid phases. Secondly, a model for the nucleation and growth of precipitates can reveal the dynamics associated with intermetallic compound formation. The nucleation and growth model developed predicts that the inhibition layer covers 99.9% of the steel surface in 0.0011 second with the iron upersaturation of 0.56wt.% and the aluminum concentration of 0.20wt.% in a molten zinc bath at 460°C.","abstract_html":"Hot-dip galvanizing (HDG) is a well-known process that increases the resistance of a steel strip to corrosion. Immersion of an automotive steel sheet in a galvanizing bath initiates a dissolution reaction. The flux of iron from the steel surface into the liquid zinc bath provides a driving force for the formation of an inhibition layer and the precipitation of dross particles. Such reactions involve the kinetics of nucleation and growth of intermetallic phases. This study addresses two main issues. First, the iron dissolution rate constant is governed by the solubility of iron in the liquid zinc under a metastable state between the pure bcc iron and the liquid phases. Secondly, a model for the nucleation and growth of precipitates can reveal the dynamics associated with intermetallic compound formation. The nucleation and growth model developed predicts that the inhibition layer covers 99.9% of the steel surface in 0.0011 second with the iron upersaturation of 0.56wt.% and the aluminum concentration of 0.20wt.% in a molten zinc bath at 460°C.","abstract_has_math":false,"creators":["Lin, Kang-Yi"],"institution":"Case Western Reserve University School of Graduate Studies","degree_name":"Master of Sciences","degree_level":"masters","degree_discipline":"Materials Science and Engineering","degree_department":null,"school":null,"contributors":["Michal, Gary"],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2011,"date_issued":"2011-09-19","date_published":"2011-09-19","updated_at":"2026-11-26T03:18:47Z","subjects":["Metallurgy","Galvanizing","CALPHAD","Iron Dissolution","Iron Solubility","Effective Aluminum","Inhibition Layer","Mass Transfer Coefficient","Dross","Computer Modeling"],"languages":["English"],"rights":["unrestricted","This thesis or dissertation is protected by copyright: some rights reserved. It is licensed for use under a Creative Commons license. Specific terms and permissions are available from this document's record in the OhioLINK ETD Center."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://rave.ohiolink.edu/etdc/view?acc_num=case1307733545","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"http://rave.ohiolink.edu/etdc/view?acc_num=case1307733545","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aohiolink%3Aoai%3Aetd.ohiolink.edu%3Acase1307733545","prefix":"oai_dc"},"source_record":{"url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Aetd.ohiolink.edu%3Acase1307733545","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor","label":"Contributor","values":["Michal, Gary"]},{"key":"dc:creator","label":"Author","values":["Lin, Kang-Yi"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2011-09-19"]},{"key":"dc:publisher","label":"Institution","values":["Case Western Reserve University School of Graduate Studies / OhioLINK"]},{"key":"dc:type","label":"Dc Type","values":["Electronic Thesis or Dissertation"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Materials Science and Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["masters"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Master of Sciences"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["Case Western Reserve University School of Graduate Studies"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Metallurgy","Galvanizing","CALPHAD","Iron Dissolution","Iron Solubility","Effective Aluminum","Inhibition Layer","Mass Transfer Coefficient","Dross","Computer Modeling"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:rights","label":"Dc Rights","values":["unrestricted","This thesis or dissertation is protected by copyright: some rights reserved. It is licensed for use under a Creative Commons license. Specific terms and permissions are available from this document's record in the OhioLINK ETD Center."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://rave.ohiolink.edu/etdc/view?acc_num=case1307733545"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["Hot-dip galvanizing (HDG) is a well-known process that increases the resistance of a steel strip to corrosion. Immersion of an automotive steel sheet in a galvanizing bath initiates a dissolution reaction. The flux of iron from the steel surface into the liquid zinc bath provides a driving force for the formation of an inhibition layer and the precipitation of dross particles. Such reactions involve the kinetics of nucleation and growth of intermetallic phases. This study addresses two main issues. First, the iron dissolution rate constant is governed by the solubility of iron in the liquid zinc under a metastable state between the pure bcc iron and the liquid phases. Secondly, a model for the nucleation and growth of precipitates can reveal the dynamics associated with intermetallic compound formation. The nucleation and growth model developed predicts that the inhibition layer covers 99.9% of the steel surface in 0.0011 second with the iron upersaturation of 0.56wt.% and the aluminum concentration of 0.20wt.% in a molten zinc bath at 460°C."]},{"key":"dc:format","label":"Dc Format","values":["application/pdf","p.92","881.2 KB"]},{"key":"dc:title","label":"Title","values":["The Dissolution of Iron from Automotive Steel Sheets in a Molten Zinc Bath and the Kinetics of the Nucleation and Growth of Dross Particles"]}]}],"canonical_facts":{"dc:contributor":["Michal, Gary"],"dc:creator":["Lin, Kang-Yi"],"dc:date":["2011-09-19"],"dc:description":["Hot-dip galvanizing (HDG) is a well-known process that increases the resistance of a steel strip to corrosion. Immersion of an automotive steel sheet in a galvanizing bath initiates a dissolution reaction. The flux of iron from the steel surface into the liquid zinc bath provides a driving force for the formation of an inhibition layer and the precipitation of dross particles. Such reactions involve the kinetics of nucleation and growth of intermetallic phases. This study addresses two main issues. First, the iron dissolution rate constant is governed by the solubility of iron in the liquid zinc under a metastable state between the pure bcc iron and the liquid phases. Secondly, a model for the nucleation and growth of precipitates can reveal the dynamics associated with intermetallic compound formation. The nucleation and growth model developed predicts that the inhibition layer covers 99.9% of the steel surface in 0.0011 second with the iron upersaturation of 0.56wt.% and the aluminum concentration of 0.20wt.% in a molten zinc bath at 460°C."],"dc:format":["application/pdf","p.92","881.2 KB"],"dc:identifier":["http://rave.ohiolink.edu/etdc/view?acc_num=case1307733545"],"dc:language":["English"],"dc:publisher":["Case Western Reserve University School of Graduate Studies / OhioLINK"],"dc:rights":["unrestricted","This thesis or dissertation is protected by copyright: some rights reserved. It is licensed for use under a Creative Commons license. Specific terms and permissions are available from this document's record in the OhioLINK ETD Center."],"dc:subject":["Metallurgy","Galvanizing","CALPHAD","Iron Dissolution","Iron Solubility","Effective Aluminum","Inhibition Layer","Mass Transfer Coefficient","Dross","Computer Modeling"],"dc:title":["The Dissolution of Iron from Automotive Steel Sheets in a Molten Zinc Bath and the Kinetics of the Nucleation and Growth of Dross Particles"],"dc:type":["Electronic Thesis or Dissertation"],"thesis:degree_discipline":["Materials Science and Engineering"],"thesis:degree_level":["masters"],"thesis:degree_name":["Master of Sciences"],"thesis:institution_name":["Case Western Reserve University School of Graduate Studies"]},"updated_at":"2026-11-26T03:18:47Z"}