{"id":{"repo_id":"ohiolink","oai_identifier":"oai:etd.ohiolink.edu:case1334239996"},"canonical_url":"https://search.ndltd.org/etd/ohiolink/oai:etd.ohiolink.edu:case1334239996","repository":{"repo_id":"ohiolink","name":"OhioLINK","base_url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai"},"display":{"title":"The Effect of Solutionizing Heat Up Rate and Quench Rate on the Grain Size and Fracture Mode of a 6061 Alloy Pressure Vessel","abstract":"Current production techniques for large diameter 6061 alloy seamless pressure vessels can lead to cylinder heads with regions of large (1mm+) grains that fracture in a low ductility intergranular fashion along the circumference of the head during proof tests. This phenomena and fracture mode was reproduced in commercially produced cylinders by a combination of slow strain rate (10-6/s) 4-point bending and controlled surface strain experiments. As-spun heads were commercially produced and given solution heat treatments at CWRU via either a salt bath or an induction coil, the former followed by quenching at rates from 180°C/s to 18°C/s. The effects of these different heat treatments on the resulting grain size, crack resistance and fracture mode were compared to the standard commercial treatments. Induction heated samples produced grain sizes below 150 µm and exhibited a significantly higher crack resistance, fracturing in a transgranular ductile manner.","abstract_html":"Current production techniques for large diameter 6061 alloy seamless pressure vessels can lead to cylinder heads with regions of large (1mm+) grains that fracture in a low ductility intergranular fashion along the circumference of the head during proof tests. This phenomena and fracture mode was reproduced in commercially produced cylinders by a combination of slow strain rate (10-6/s) 4-point bending and controlled surface strain experiments. As-spun heads were commercially produced and given solution heat treatments at CWRU via either a salt bath or an induction coil, the former followed by quenching at rates from 180°C/s to 18°C/s. The effects of these different heat treatments on the resulting grain size, crack resistance and fracture mode were compared to the standard commercial treatments. Induction heated samples produced grain sizes below 150 µm and exhibited a significantly higher crack resistance, fracturing in a transgranular ductile manner.","abstract_has_math":false,"creators":["Kulpinski, Kyle E."],"institution":"Case Western Reserve University School of Graduate Studies","degree_name":"Master of Sciences (Engineering)","degree_level":"masters","degree_discipline":"Materials Science and Engineering","degree_department":null,"school":null,"contributors":["Lewandowski, John"],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2012,"date_issued":"2012-06-26","date_published":"2012-06-26","updated_at":"2026-11-26T03:19:02Z","subjects":["Aerospace Materials","Materials Science","Metallurgy","aluminum","grain growth","pressure vessel","fracture","solution heat treatment","heat treatment"],"languages":["English"],"rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://rave.ohiolink.edu/etdc/view?acc_num=case1334239996","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"http://rave.ohiolink.edu/etdc/view?acc_num=case1334239996","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aohiolink%3Aoai%3Aetd.ohiolink.edu%3Acase1334239996","prefix":"oai_dc"},"source_record":{"url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Aetd.ohiolink.edu%3Acase1334239996","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor","label":"Contributor","values":["Lewandowski, John"]},{"key":"dc:creator","label":"Author","values":["Kulpinski, Kyle E."]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2012-06-26"]},{"key":"dc:publisher","label":"Institution","values":["Case Western Reserve University School of Graduate Studies / OhioLINK"]},{"key":"dc:type","label":"Dc Type","values":["Electronic Thesis or Dissertation"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Materials Science and Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["masters"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Master of Sciences (Engineering)"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["Case Western Reserve University School of Graduate Studies"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Aerospace Materials","Materials Science","Metallurgy","aluminum","grain growth","pressure vessel","fracture","solution heat treatment","heat treatment"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:rights","label":"Dc Rights","values":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://rave.ohiolink.edu/etdc/view?acc_num=case1334239996"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["Current production techniques for large diameter 6061 alloy seamless pressure vessels can lead to cylinder heads with regions of large (1mm+) grains that fracture in a low ductility intergranular fashion along the circumference of the head during proof tests. This phenomena and fracture mode was reproduced in commercially produced cylinders by a combination of slow strain rate (10-6/s) 4-point bending and controlled surface strain experiments. As-spun heads were commercially produced and given solution heat treatments at CWRU via either a salt bath or an induction coil, the former followed by quenching at rates from 180°C/s to 18°C/s. The effects of these different heat treatments on the resulting grain size, crack resistance and fracture mode were compared to the standard commercial treatments. Induction heated samples produced grain sizes below 150 µm and exhibited a significantly higher crack resistance, fracturing in a transgranular ductile manner."]},{"key":"dc:format","label":"Dc Format","values":["application/pdf","12.38 MB"]},{"key":"dc:title","label":"Title","values":["The Effect of Solutionizing Heat Up Rate and Quench Rate on the Grain Size and Fracture Mode of a 6061 Alloy Pressure Vessel"]}]}],"canonical_facts":{"dc:contributor":["Lewandowski, John"],"dc:creator":["Kulpinski, Kyle E."],"dc:date":["2012-06-26"],"dc:description":["Current production techniques for large diameter 6061 alloy seamless pressure vessels can lead to cylinder heads with regions of large (1mm+) grains that fracture in a low ductility intergranular fashion along the circumference of the head during proof tests. This phenomena and fracture mode was reproduced in commercially produced cylinders by a combination of slow strain rate (10-6/s) 4-point bending and controlled surface strain experiments. As-spun heads were commercially produced and given solution heat treatments at CWRU via either a salt bath or an induction coil, the former followed by quenching at rates from 180°C/s to 18°C/s. The effects of these different heat treatments on the resulting grain size, crack resistance and fracture mode were compared to the standard commercial treatments. Induction heated samples produced grain sizes below 150 µm and exhibited a significantly higher crack resistance, fracturing in a transgranular ductile manner."],"dc:format":["application/pdf","12.38 MB"],"dc:identifier":["http://rave.ohiolink.edu/etdc/view?acc_num=case1334239996"],"dc:language":["English"],"dc:publisher":["Case Western Reserve University School of Graduate Studies / OhioLINK"],"dc:rights":["unrestricted","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"dc:subject":["Aerospace Materials","Materials Science","Metallurgy","aluminum","grain growth","pressure vessel","fracture","solution heat treatment","heat treatment"],"dc:title":["The Effect of Solutionizing Heat Up Rate and Quench Rate on the Grain Size and Fracture Mode of a 6061 Alloy Pressure Vessel"],"dc:type":["Electronic Thesis or Dissertation"],"thesis:degree_discipline":["Materials Science and Engineering"],"thesis:degree_level":["masters"],"thesis:degree_name":["Master of Sciences (Engineering)"],"thesis:institution_name":["Case Western Reserve University School of Graduate Studies"]},"updated_at":"2026-11-26T03:19:02Z"}