{"id":{"repo_id":"ohiolink","oai_identifier":"oai:etd.ohiolink.edu:ucin998071429"},"canonical_url":"https://search.ndltd.org/etd/ohiolink/oai:etd.ohiolink.edu:ucin998071429","repository":{"repo_id":"ohiolink","name":"OhioLINK","base_url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai"},"display":{"title":"INTERFACIAL MODIFICATION FOR THE REINFORCEMENT OF SILICONE ELASTOMER COMPOSITES","abstract":"Interfacial modification of silicone elastomer composites is studied to enhance the understanding of the mechanism of the reinforcement and to develop improved materials. Information on the phase structure and interface structure were obtained from Ultra Small and Small Angle X-ray Scattering measurements (USAXS and SAXS). Stress-strain measurements were carried out on these elastomeric composites to yield values of the tensile modulus, tensile strength and toughness. The surface areas of fillers were measured by nitrogen absorption (Brunauer-Emmett-Teller). Fourier Transformed Infrared (FTIR) was employed to characterize surface properties of the fillers and crosslinking reactions. Scanning electron microcopy (SEM) was used to characterize the morphology of the fillers and composites. The object of the first section is to synthesize composites having modified interfaces based on vinyltrimethoxysilane (VTS) and vinylmethyldimethoxysilane (VMDS) to bond durably the silica fillers to the polydimethysiloxane (PDMS) networks. Silica fillers were generated by the in-situ method. The effect of coupling agents on the phase structure was investigated experimentally. The concentration of coupling agents governs the domain size of silica fillers, as increase in amounts of coupling agent leads to decrease in domain size, consequently resulting in higher surface area and stronger filler-polymer interaction. Compared to vinylmethyldimethoxysilane, vinyltrimethoxysilane shows enhanced control of the chemical growth of silica within elastomer network. Equilibrium stress-strain and non-equilibrium tensile stress-strain measurements were carried out on the synthesized composites to investigate the effect of the resulting structure on mechanical properties. The modified-interface composites had better mechanical properties, compared to their unmodified counterparts. At the same silica loading level, the composites containing higher concentration of coupling agent (in the range of 0-5 wt %) had better mechanical properties. The second section deals with the composites having irreversible and reversible interfacial bonding between the two phases. The reversible interfaces contain hemiacetal ester that would dissociate at about 120°C to 150°C, while the irreversible interfacial bonding contains azo groups that would be broken over 60°C. Compared to the hemi and azo composites, the unmodified SiO <sub>2</sub> /PDMS composites had higher modulus at 5 and 10 wt % of filler, presumably due to higher surface area of silica fillers and stronger filler-filler interactions. However, the hemi and azo composites had higher ultimate stress and elongation, and better toughness. For hemi and azo composites, the extensibility of the elastomers increased when more filler is introduced.","abstract_html":"Interfacial modification of silicone elastomer composites is studied to enhance the understanding of the mechanism of the reinforcement and to develop improved materials. Information on the phase structure and interface structure were obtained from Ultra Small and Small Angle X-ray Scattering measurements (USAXS and SAXS). Stress-strain measurements were carried out on these elastomeric composites to yield values of the tensile modulus, tensile strength and toughness. The surface areas of fillers were measured by nitrogen absorption (Brunauer-Emmett-Teller). Fourier Transformed Infrared (FTIR) was employed to characterize surface properties of the fillers and crosslinking reactions. Scanning electron microcopy (SEM) was used to characterize the morphology of the fillers and composites. The object of the first section is to synthesize composites having modified interfaces based on vinyltrimethoxysilane (VTS) and vinylmethyldimethoxysilane (VMDS) to bond durably the silica fillers to the polydimethysiloxane (PDMS) networks. Silica fillers were generated by the in-situ method. The effect of coupling agents on the phase structure was investigated experimentally. The concentration of coupling agents governs the domain size of silica fillers, as increase in amounts of coupling agent leads to decrease in domain size, consequently resulting in higher surface area and stronger filler-polymer interaction. Compared to vinylmethyldimethoxysilane, vinyltrimethoxysilane shows enhanced control of the chemical growth of silica within elastomer network. Equilibrium stress-strain and non-equilibrium tensile stress-strain measurements were carried out on the synthesized composites to investigate the effect of the resulting structure on mechanical properties. The modified-interface composites had better mechanical properties, compared to their unmodified counterparts. At the same silica loading level, the composites containing higher concentration of coupling agent (in the range of 0-5 wt %) had better mechanical properties. The second section deals with the composites having irreversible and reversible interfacial bonding between the two phases. The reversible interfaces contain hemiacetal ester that would dissociate at about 120°C to 150°C, while the irreversible interfacial bonding contains azo groups that would be broken over 60°C. Compared to the hemi and azo composites, the unmodified SiO &lt;sub&gt;2&lt;/sub&gt; /PDMS composites had higher modulus at 5 and 10 wt % of filler, presumably due to higher surface area of silica fillers and stronger filler-filler interactions. However, the hemi and azo composites had higher ultimate stress and elongation, and better toughness. For hemi and azo composites, the extensibility of the elastomers increased when more filler is introduced.","abstract_has_math":false,"creators":["Vu, Bich Thi Ngoc"],"institution":"University of Cincinnati","degree_name":"MS","degree_level":"masters","degree_discipline":"Arts and Sciences : Chemistry","degree_department":null,"school":null,"contributors":[],"advisors":["Mark, James"],"committee_chairs":[],"committee_members":[],"year":2001,"date_issued":"2001-10-11","date_published":"2001-10-11","updated_at":"2026-11-27T04:38:26Z","subjects":["ELASTOMER COMPOSITES","REVERSIBLE INTERFACE","SMALL ANGLE X-RAY SCATTERING","POLYDIMETHYLSILOXANE REINFORCEMENT","COUPLING AGENTS"],"languages":["English"],"rights":["restricted--full text not available online","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://rave.ohiolink.edu/etdc/view?acc_num=ucin998071429","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"http://rave.ohiolink.edu/etdc/view?acc_num=ucin998071429","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aohiolink%3Aoai%3Aetd.ohiolink.edu%3Aucin998071429","prefix":"oai_dc"},"source_record":{"url":"https://etd.ohiolink.edu/acprod/odb_etd/ws/oai/oai?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Aetd.ohiolink.edu%3Aucin998071429","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Mark, James"]},{"key":"dc:creator","label":"Author","values":["Vu, Bich Thi Ngoc"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2001-10-11"]},{"key":"dc:publisher","label":"Institution","values":["University of Cincinnati / OhioLINK"]},{"key":"dc:type","label":"Dc Type","values":["Electronic Thesis or Dissertation"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Arts and Sciences : Chemistry"]},{"key":"thesis:degree_level","label":"Degree Level","values":["masters"]},{"key":"thesis:degree_name","label":"Degree Name","values":["MS"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["University of Cincinnati"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["ELASTOMER COMPOSITES","REVERSIBLE INTERFACE","SMALL ANGLE X-RAY SCATTERING","POLYDIMETHYLSILOXANE REINFORCEMENT","COUPLING AGENTS"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:rights","label":"Dc Rights","values":["restricted--full text not available online","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://rave.ohiolink.edu/etdc/view?acc_num=ucin998071429"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["Interfacial modification of silicone elastomer composites is studied to enhance the understanding of the mechanism of the reinforcement and to develop improved materials. Information on the phase structure and interface structure were obtained from Ultra Small and Small Angle X-ray Scattering measurements (USAXS and SAXS). Stress-strain measurements were carried out on these elastomeric composites to yield values of the tensile modulus, tensile strength and toughness. The surface areas of fillers were measured by nitrogen absorption (Brunauer-Emmett-Teller). Fourier Transformed Infrared (FTIR) was employed to characterize surface properties of the fillers and crosslinking reactions. Scanning electron microcopy (SEM) was used to characterize the morphology of the fillers and composites. The object of the first section is to synthesize composites having modified interfaces based on vinyltrimethoxysilane (VTS) and vinylmethyldimethoxysilane (VMDS) to bond durably the silica fillers to the polydimethysiloxane (PDMS) networks. Silica fillers were generated by the in-situ method. The effect of coupling agents on the phase structure was investigated experimentally. The concentration of coupling agents governs the domain size of silica fillers, as increase in amounts of coupling agent leads to decrease in domain size, consequently resulting in higher surface area and stronger filler-polymer interaction. Compared to vinylmethyldimethoxysilane, vinyltrimethoxysilane shows enhanced control of the chemical growth of silica within elastomer network. Equilibrium stress-strain and non-equilibrium tensile stress-strain measurements were carried out on the synthesized composites to investigate the effect of the resulting structure on mechanical properties. The modified-interface composites had better mechanical properties, compared to their unmodified counterparts. At the same silica loading level, the composites containing higher concentration of coupling agent (in the range of 0-5 wt %) had better mechanical properties. The second section deals with the composites having irreversible and reversible interfacial bonding between the two phases. The reversible interfaces contain hemiacetal ester that would dissociate at about 120°C to 150°C, while the irreversible interfacial bonding contains azo groups that would be broken over 60°C. Compared to the hemi and azo composites, the unmodified SiO <sub>2</sub> /PDMS composites had higher modulus at 5 and 10 wt % of filler, presumably due to higher surface area of silica fillers and stronger filler-filler interactions. However, the hemi and azo composites had higher ultimate stress and elongation, and better toughness. For hemi and azo composites, the extensibility of the elastomers increased when more filler is introduced."]},{"key":"dc:format","label":"Dc Format","values":["application/pdf"]},{"key":"dc:title","label":"Title","values":["INTERFACIAL MODIFICATION FOR THE REINFORCEMENT OF SILICONE ELASTOMER COMPOSITES"]}]}],"canonical_facts":{"dc:contributor.advisor":["Mark, James"],"dc:creator":["Vu, Bich Thi Ngoc"],"dc:date":["2001-10-11"],"dc:description":["Interfacial modification of silicone elastomer composites is studied to enhance the understanding of the mechanism of the reinforcement and to develop improved materials. Information on the phase structure and interface structure were obtained from Ultra Small and Small Angle X-ray Scattering measurements (USAXS and SAXS). Stress-strain measurements were carried out on these elastomeric composites to yield values of the tensile modulus, tensile strength and toughness. The surface areas of fillers were measured by nitrogen absorption (Brunauer-Emmett-Teller). Fourier Transformed Infrared (FTIR) was employed to characterize surface properties of the fillers and crosslinking reactions. Scanning electron microcopy (SEM) was used to characterize the morphology of the fillers and composites. The object of the first section is to synthesize composites having modified interfaces based on vinyltrimethoxysilane (VTS) and vinylmethyldimethoxysilane (VMDS) to bond durably the silica fillers to the polydimethysiloxane (PDMS) networks. Silica fillers were generated by the in-situ method. The effect of coupling agents on the phase structure was investigated experimentally. The concentration of coupling agents governs the domain size of silica fillers, as increase in amounts of coupling agent leads to decrease in domain size, consequently resulting in higher surface area and stronger filler-polymer interaction. Compared to vinylmethyldimethoxysilane, vinyltrimethoxysilane shows enhanced control of the chemical growth of silica within elastomer network. Equilibrium stress-strain and non-equilibrium tensile stress-strain measurements were carried out on the synthesized composites to investigate the effect of the resulting structure on mechanical properties. The modified-interface composites had better mechanical properties, compared to their unmodified counterparts. At the same silica loading level, the composites containing higher concentration of coupling agent (in the range of 0-5 wt %) had better mechanical properties. The second section deals with the composites having irreversible and reversible interfacial bonding between the two phases. The reversible interfaces contain hemiacetal ester that would dissociate at about 120°C to 150°C, while the irreversible interfacial bonding contains azo groups that would be broken over 60°C. Compared to the hemi and azo composites, the unmodified SiO <sub>2</sub> /PDMS composites had higher modulus at 5 and 10 wt % of filler, presumably due to higher surface area of silica fillers and stronger filler-filler interactions. However, the hemi and azo composites had higher ultimate stress and elongation, and better toughness. For hemi and azo composites, the extensibility of the elastomers increased when more filler is introduced."],"dc:format":["application/pdf"],"dc:identifier":["http://rave.ohiolink.edu/etdc/view?acc_num=ucin998071429"],"dc:language":["English"],"dc:publisher":["University of Cincinnati / OhioLINK"],"dc:rights":["restricted--full text not available online","This thesis or dissertation is protected by copyright: all rights reserved. It may not be copied or redistributed beyond the terms of applicable copyright laws."],"dc:subject":["ELASTOMER COMPOSITES","REVERSIBLE INTERFACE","SMALL ANGLE X-RAY SCATTERING","POLYDIMETHYLSILOXANE REINFORCEMENT","COUPLING AGENTS"],"dc:title":["INTERFACIAL MODIFICATION FOR THE REINFORCEMENT OF SILICONE ELASTOMER COMPOSITES"],"dc:type":["Electronic Thesis or Dissertation"],"thesis:degree_discipline":["Arts and Sciences : Chemistry"],"thesis:degree_level":["masters"],"thesis:degree_name":["MS"],"thesis:institution_name":["University of Cincinnati"]},"updated_at":"2026-11-27T04:38:26Z"}