{"id":{"repo_id":"pohang","oai_identifier":"oai:oasis.postech.ac.kr:2014.oak/1599"},"canonical_url":"https://search.ndltd.org/etd/pohang/oai:oasis.postech.ac.kr:2014.oak/1599","repository":{"repo_id":"pohang","name":"Pohang University of Science and Technology","base_url":"http://oasis.postech.ac.kr/oai/request"},"display":{"title":"Use of Thermodynamic Calculations in Predicting the Corrosion Behavior of Refractories for Steelmaking","abstract":"Refractories are non-metallic materials used to line many industrial furnaces for the high temperature production of other materials such as metals, glass, cement, and petrochemicals. Decreased service life of refractories is caused by damage arising from, for example, deformation at high temperature, thermal shock, mechanical abrasion, and chemical corrosion. Among these factors, chemical attack by molten steel or slag is often the most critical. To determine chemical corrosion mechanisms and to compare corrosion behavior of different refractories, several test methods(rotary corrosion test, crucible test, high frequency induction furnace test, et al.) have evolved. However, many of these tests are expensive and time consuming, and in some cases, they are conducted just to re-establish information already known and generally available in existing phase diagrams. In the present study, the utilization of thermodynamic calculations is proposed to predict the corrosion behavior of refractories for steelmaking (especially, RH process and continuous casting process). At part 1, we proposed the effective equilibrium reaction zone model to predict the complex industrial RH process using thermodynamic calculations. In this approach, all phases within the \"effective\" reaction zone located at a reaction interface are assumed to reach equilibrium. The results of the model were used to clarify the decarburization behavior observed during the RH process. According to the model predictions, the RH slag contains a high FetO level during the first 15min of the RH process. During the Al addition, the reducible components in the slag including FetO, SiO2, MnO and CrOX are reduced by Al. After the Al addition, the RH slag becomes a CaO-Al2O3 slag containing some MgO. Five slag compositions were selected to simulate the major slag composition changes in the RH vessel during the degassing process","abstract_html":"Refractories are non-metallic materials used to line many industrial furnaces for the high temperature production of other materials such as metals, glass, cement, and petrochemicals. Decreased service life of refractories is caused by damage arising from, for example, deformation at high temperature, thermal shock, mechanical abrasion, and chemical corrosion. Among these factors, chemical attack by molten steel or slag is often the most critical. To determine chemical corrosion mechanisms and to compare corrosion behavior of different refractories, several test methods(rotary corrosion test, crucible test, high frequency induction furnace test, et al.) have evolved. However, many of these tests are expensive and time consuming, and in some cases, they are conducted just to re-establish information already known and generally available in existing phase diagrams. In the present study, the utilization of thermodynamic calculations is proposed to predict the corrosion behavior of refractories for steelmaking (especially, RH process and continuous casting process). At part 1, we proposed the effective equilibrium reaction zone model to predict the complex industrial RH process using thermodynamic calculations. In this approach, all phases within the &quot;effective&quot; reaction zone located at a reaction interface are assumed to reach equilibrium. The results of the model were used to clarify the decarburization behavior observed during the RH process. According to the model predictions, the RH slag contains a high FetO level during the first 15min of the RH process. During the Al addition, the reducible components in the slag including FetO, SiO2, MnO and CrOX are reduced by Al. After the Al addition, the RH slag becomes a CaO-Al2O3 slag containing some MgO. Five slag compositions were selected to simulate the major slag composition changes in the RH vessel during the degassing process","abstract_has_math":false,"creators":["조문규"],"institution":null,"degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2012,"date_issued":"2012","date_published":"2012","updated_at":"2026-11-26T04:05:31Z","subjects":[],"languages":[],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["hdl:2014.oak/1599"],"render_values":[{"text":"hdl:2014.oak/1599","href":null,"code":true}]},{"key":"mods:identifier.other","label":"Mods Identifier Other","values":["OAK-2014-01097"],"render_values":[{"text":"OAK-2014-01097","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":"http://postech.dcollection.net/jsp/common/DcLoOrgPer.jsp?sItemId=000001384754","outbound_label":"Repository record","outbound_source":"mods:identifier.uri","record_url":"http://postech.dcollection.net/jsp/common/DcLoOrgPer.jsp?sItemId=000001384754","record_label":"Repository record","record_kind":"record","record_source":"mods:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Apohang%3Aoai%3Aoasis.postech.ac.kr%3A2014.oak%2F1599","prefix":"oai_dc"},"source_record":{"url":"http://oasis.postech.ac.kr/oai/request?verb=GetRecord&metadataPrefix=mets&identifier=oai%3Aoasis.postech.ac.kr%3A2014.oak%2F1599","prefix":"mets"},"metadata_groups":[{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.issued","label":"Date","values":["2012"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["hdl:2014.oak/1599"]},{"key":"mods:identifier.other","label":"Mods Identifier Other","values":["OAK-2014-01097"]},{"key":"mods:identifier.uri","label":"Mods Identifier URI","values":["http://postech.dcollection.net/jsp/common/DcLoOrgPer.jsp?sItemId=000001384754"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.other","label":"Dc Description Other","values":["Refractories are non-metallic materials used to line many industrial furnaces for the high temperature production of other materials such as metals, glass, cement, and petrochemicals. Decreased service life of refractories is caused by damage arising from, for example, deformation at high temperature, thermal shock, mechanical abrasion, and chemical corrosion. Among these factors, chemical attack by molten steel or slag is often the most critical. To determine chemical corrosion mechanisms and to compare corrosion behavior of different refractories, several test methods(rotary corrosion test, crucible test, high frequency induction furnace test, et al.) have evolved. However, many of these tests are expensive and time consuming, and in some cases, they are conducted just to re-establish information already known and generally available in existing phase diagrams. In the present study, the utilization of thermodynamic calculations is proposed to predict the corrosion behavior of refractories for steelmaking (especially, RH process and continuous casting process). At part 1, we proposed the effective equilibrium reaction zone model to predict the complex industrial RH process using thermodynamic calculations. In this approach, all phases within the \"effective\" reaction zone located at a reaction interface are assumed to reach equilibrium. The results of the model were used to clarify the decarburization behavior observed during the RH process. According to the model predictions, the RH slag contains a high FetO level during the first 15min of the RH process. During the Al addition, the reducible components in the slag including FetO, SiO2, MnO and CrOX are reduced by Al. After the Al addition, the RH slag becomes a CaO-Al2O3 slag containing some MgO. Five slag compositions were selected to simulate the major slag composition changes in the RH vessel during the degassing process"]},{"key":"dc:title","label":"Title","values":["Use of Thermodynamic Calculations in Predicting the Corrosion Behavior of Refractories for Steelmaking"]},{"key":"mods:accesscondition.useandreproduction","label":"Mods Accesscondition Useandreproduction","values":["BY_NC_ND"]},{"key":"mods:dateaccessioned","label":"Mods Dateaccessioned","values":["2014-12-01T11:48:12Z"]},{"key":"mods:dateavailable","label":"Mods Dateavailable","values":["2014-12-01T11:48:12Z"]},{"key":"mods:namepart","label":"Mods Namepart","values":["조문규","일반대학원 신소재공학과","포항공과대학교"]},{"key":"mods:roleterm.text","label":"Mods Roleterm Text","values":["author","college","department"]}]}],"canonical_facts":{"dc:date.issued":["2012"],"dc:description.other":["Refractories are non-metallic materials used to line many industrial furnaces for the high temperature production of other materials such as metals, glass, cement, and petrochemicals. Decreased service life of refractories is caused by damage arising from, for example, deformation at high temperature, thermal shock, mechanical abrasion, and chemical corrosion. Among these factors, chemical attack by molten steel or slag is often the most critical. To determine chemical corrosion mechanisms and to compare corrosion behavior of different refractories, several test methods(rotary corrosion test, crucible test, high frequency induction furnace test, et al.) have evolved. However, many of these tests are expensive and time consuming, and in some cases, they are conducted just to re-establish information already known and generally available in existing phase diagrams. In the present study, the utilization of thermodynamic calculations is proposed to predict the corrosion behavior of refractories for steelmaking (especially, RH process and continuous casting process). At part 1, we proposed the effective equilibrium reaction zone model to predict the complex industrial RH process using thermodynamic calculations. In this approach, all phases within the \"effective\" reaction zone located at a reaction interface are assumed to reach equilibrium. The results of the model were used to clarify the decarburization behavior observed during the RH process. According to the model predictions, the RH slag contains a high FetO level during the first 15min of the RH process. During the Al addition, the reducible components in the slag including FetO, SiO2, MnO and CrOX are reduced by Al. After the Al addition, the RH slag becomes a CaO-Al2O3 slag containing some MgO. Five slag compositions were selected to simulate the major slag composition changes in the RH vessel during the degassing process"],"dc:identifier":["hdl:2014.oak/1599"],"dc:title":["Use of Thermodynamic Calculations in Predicting the Corrosion Behavior of Refractories for Steelmaking"],"dc:type":["Thesis"],"mods:accesscondition.useandreproduction":["BY_NC_ND"],"mods:dateaccessioned":["2014-12-01T11:48:12Z"],"mods:dateavailable":["2014-12-01T11:48:12Z"],"mods:identifier.other":["OAK-2014-01097"],"mods:identifier.uri":["http://postech.dcollection.net/jsp/common/DcLoOrgPer.jsp?sItemId=000001384754"],"mods:namepart":["조문규","일반대학원 신소재공학과","포항공과대학교"],"mods:roleterm.text":["author","college","department"]},"updated_at":"2026-11-26T04:05:31Z"}