{"id":{"repo_id":"purdue-thes","oai_identifier":"oai:docs.lib.purdue.edu:open_access_dissertations-3040"},"canonical_url":"https://search.ndltd.org/etd/purdue-thes/oai:docs.lib.purdue.edu:open_access_dissertations-3040","repository":{"repo_id":"purdue-thes","name":"Purdue University","base_url":"https://docs.lib.purdue.edu/do/oai/"},"display":{"title":"Strength and Serviceability of Concrete Elements Reinforced with High-Strength Steel","abstract":"The potential use of high-strength steel reinforcement (HSSR) with yield stress (𝑓𝑦) larger than 80 ksi requires reconsideration of design criteria and limits used to avoid sudden failure because they were conceived for elements with Gr. 60 and 80 (𝑓𝑦=60 and 80 ksi) reinforcement. The objective of this study is to investigate the feasibility of using HSSR for applications not related to seismic demands, with a focus on three topics: (i) minimum flexural reinforcement in slabs and walls, (ii) maximum flexural reinforcement in beams, and (iii) crack widths and deflections. Nine slabs with gross longitudinal reinforcement ratio (𝜌𝑔) between 0.07% and 0.18%, four walls with 𝜌𝑔 between 0.07% and 0.24%, and six continuous beams with longitudinal reinforcement ratio between 0.8% and 2.5% and a net tensile strain of approximately 0.005 were tested to study the strength, toughness, and serviceability of elements with HSSR. The test data indicated that it is feasible to use HSSR (with 𝑓𝑦 up to 120 ksi). The following conclusions are made in relation to the three specific topics investigated: 1) Minimum longitudinal reinforcement ratio for slabs can be reduced in inverse proportion to increase in yield stress. Test slabs with HSSR and 𝜌𝑔 as small as 0.09% had rotational capacities larger than 4%. Nevertheless prudence is due because brittle failure may occur at small displacements in lightly reinforced elements in which cracking moment approaches or exceeds yield moment and because low shear strength has been observed to be associated with low ratios of longitudinal reinforcement. 2) Current minimum longitudinal reinforcement limits in walls with uniformly distributed reinforcement, even for Gr.60 reinforcement, should be reconsidered. Specimens with Gr. 60 and Gr.120 bars, and 𝜌𝑔 ranging between 0.07% and 0.24% failed at drift capacities smaller than 1%. In walls with products of gross reinforcement ratio and measured yield stress smaller than approximately 200 psi, failure took place just after first cracking and at loads smaller than those at first cracking suggesting that elements in this range should be avoided in all structures no matter how low the probability of cracking is estimated to be. This is especially critical for ordinary structural walls without confined boundary elements in seismic regions. 3) In the tests conducted, sections with HSSR designed to have net tensile strain (𝜀𝑡) of 0.005 had sufficient rotational capacity for moment redistribution. In design, detailing to accommodate increases in shear and bond demands caused by load redistribution is needed and may be as critical as controlling maximum reinforcement ratio through 𝜀𝑡 to avoid brittle failure. 4) Test data suggest that extrapolation of minimum thickness for one-way slabs with HSSR as the thickness required for an element with working stress of 40 ksi multiplied by a factor related to working stress in the reinforcing bars (𝑓𝑠), 0.4+ 3𝑓𝑠(𝑘𝑠𝑖)200𝑘𝑠𝑖 , would lead to acceptable immediate and long-term deflections. 5) According to the measurements made, reduction in bar spacing (s) with increase in working stress in the reinforcing bars (𝑓𝑠), determined as 𝑠=15(40,000𝑓𝑠(𝑝𝑠𝑖))−2.5∗𝑐𝑜𝑣𝑒𝑟, would be sufficient to avoid intolerable crack widths even in elements with working stresses up to 80 ksi.","abstract_html":"The potential use of high-strength steel reinforcement (HSSR) with yield stress (𝑓𝑦) larger than 80 ksi requires reconsideration of design criteria and limits used to avoid sudden failure because they were conceived for elements with Gr. 60 and 80 (𝑓𝑦=60 and 80 ksi) reinforcement. The objective of this study is to investigate the feasibility of using HSSR for applications not related to seismic demands, with a focus on three topics: (i) minimum flexural reinforcement in slabs and walls, (ii) maximum flexural reinforcement in beams, and (iii) crack widths and deflections. Nine slabs with gross longitudinal reinforcement ratio (𝜌𝑔) between 0.07% and 0.18%, four walls with 𝜌𝑔 between 0.07% and 0.24%, and six continuous beams with longitudinal reinforcement ratio between 0.8% and 2.5% and a net tensile strain of approximately 0.005 were tested to study the strength, toughness, and serviceability of elements with HSSR. The test data indicated that it is feasible to use HSSR (with 𝑓𝑦 up to 120 ksi). The following conclusions are made in relation to the three specific topics investigated: 1) Minimum longitudinal reinforcement ratio for slabs can be reduced in inverse proportion to increase in yield stress. Test slabs with HSSR and 𝜌𝑔 as small as 0.09% had rotational capacities larger than 4%. Nevertheless prudence is due because brittle failure may occur at small displacements in lightly reinforced elements in which cracking moment approaches or exceeds yield moment and because low shear strength has been observed to be associated with low ratios of longitudinal reinforcement. 2) Current minimum longitudinal reinforcement limits in walls with uniformly distributed reinforcement, even for Gr.60 reinforcement, should be reconsidered. Specimens with Gr. 60 and Gr.120 bars, and 𝜌𝑔 ranging between 0.07% and 0.24% failed at drift capacities smaller than 1%. In walls with products of gross reinforcement ratio and measured yield stress smaller than approximately 200 psi, failure took place just after first cracking and at loads smaller than those at first cracking suggesting that elements in this range should be avoided in all structures no matter how low the probability of cracking is estimated to be. This is especially critical for ordinary structural walls without confined boundary elements in seismic regions. 3) In the tests conducted, sections with HSSR designed to have net tensile strain (𝜀𝑡) of 0.005 had sufficient rotational capacity for moment redistribution. In design, detailing to accommodate increases in shear and bond demands caused by load redistribution is needed and may be as critical as controlling maximum reinforcement ratio through 𝜀𝑡 to avoid brittle failure. 4) Test data suggest that extrapolation of minimum thickness for one-way slabs with HSSR as the thickness required for an element with working stress of 40 ksi multiplied by a factor related to working stress in the reinforcing bars (𝑓𝑠), 0.4+ 3𝑓𝑠(𝑘𝑠𝑖)200𝑘𝑠𝑖 , would lead to acceptable immediate and long-term deflections. 5) According to the measurements made, reduction in bar spacing (s) with increase in working stress in the reinforcing bars (𝑓𝑠), determined as 𝑠=15(40,000𝑓𝑠(𝑝𝑠𝑖))−2.5∗𝑐𝑜𝑣𝑒𝑟, would be sufficient to avoid intolerable crack widths even in elements with working stresses up to 80 ksi.","abstract_has_math":false,"creators":["Puranam, Aishwarya Y."],"institution":null,"degree_name":"Doctor of Philosophy (PhD)","degree_level":"Dissertation","degree_discipline":"Civil Engineering","degree_department":null,"school":null,"contributors":["Santiago Pujol","Ayhan Irfanoglu","Julio Ramirez","Duly Abraham"],"advisors":[],"committee_chairs":[],"committee_members":[],"year":null,"date_issued":"","date_published":null,"updated_at":"2026-11-19T08:51:41Z","subjects":[],"languages":[],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"https://docs.lib.purdue.edu/open_access_dissertations/1803","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"https://docs.lib.purdue.edu/open_access_dissertations/1803","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","download_url":null,"download_label":null,"download_source":null,"access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://docs.lib.purdue.edu/do/oai/?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Adocs.lib.purdue.edu%3Aopen_access_dissertations-3040","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor","label":"Contributor","values":["Santiago Pujol","Ayhan Irfanoglu","Julio Ramirez","Duly Abraham"]},{"key":"dc:creator","label":"Author","values":["Puranam, Aishwarya Y."]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.created","label":"Dc Date Created","values":["2018-05-01T07:00:00Z"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Civil Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["Dissertation"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Doctor of Philosophy (PhD)"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["https://docs.lib.purdue.edu/open_access_dissertations/1803"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["The potential use of high-strength steel reinforcement (HSSR) with yield stress (𝑓𝑦) larger than 80 ksi requires reconsideration of design criteria and limits used to avoid sudden failure because they were conceived for elements with Gr. 60 and 80 (𝑓𝑦=60 and 80 ksi) reinforcement. The objective of this study is to investigate the feasibility of using HSSR for applications not related to seismic demands, with a focus on three topics: (i) minimum flexural reinforcement in slabs and walls, (ii) maximum flexural reinforcement in beams, and (iii) crack widths and deflections. Nine slabs with gross longitudinal reinforcement ratio (𝜌𝑔) between 0.07% and 0.18%, four walls with 𝜌𝑔 between 0.07% and 0.24%, and six continuous beams with longitudinal reinforcement ratio between 0.8% and 2.5% and a net tensile strain of approximately 0.005 were tested to study the strength, toughness, and serviceability of elements with HSSR. The test data indicated that it is feasible to use HSSR (with 𝑓𝑦 up to 120 ksi). The following conclusions are made in relation to the three specific topics investigated: 1) Minimum longitudinal reinforcement ratio for slabs can be reduced in inverse proportion to increase in yield stress. Test slabs with HSSR and 𝜌𝑔 as small as 0.09% had rotational capacities larger than 4%. Nevertheless prudence is due because brittle failure may occur at small displacements in lightly reinforced elements in which cracking moment approaches or exceeds yield moment and because low shear strength has been observed to be associated with low ratios of longitudinal reinforcement. 2) Current minimum longitudinal reinforcement limits in walls with uniformly distributed reinforcement, even for Gr.60 reinforcement, should be reconsidered. Specimens with Gr. 60 and Gr.120 bars, and 𝜌𝑔 ranging between 0.07% and 0.24% failed at drift capacities smaller than 1%. In walls with products of gross reinforcement ratio and measured yield stress smaller than approximately 200 psi, failure took place just after first cracking and at loads smaller than those at first cracking suggesting that elements in this range should be avoided in all structures no matter how low the probability of cracking is estimated to be. This is especially critical for ordinary structural walls without confined boundary elements in seismic regions. 3) In the tests conducted, sections with HSSR designed to have net tensile strain (𝜀𝑡) of 0.005 had sufficient rotational capacity for moment redistribution. In design, detailing to accommodate increases in shear and bond demands caused by load redistribution is needed and may be as critical as controlling maximum reinforcement ratio through 𝜀𝑡 to avoid brittle failure. 4) Test data suggest that extrapolation of minimum thickness for one-way slabs with HSSR as the thickness required for an element with working stress of 40 ksi multiplied by a factor related to working stress in the reinforcing bars (𝑓𝑠), 0.4+ 3𝑓𝑠(𝑘𝑠𝑖)200𝑘𝑠𝑖 , would lead to acceptable immediate and long-term deflections. 5) According to the measurements made, reduction in bar spacing (s) with increase in working stress in the reinforcing bars (𝑓𝑠), determined as 𝑠=15(40,000𝑓𝑠(𝑝𝑠𝑖))−2.5∗𝑐𝑜𝑣𝑒𝑟, would be sufficient to avoid intolerable crack widths even in elements with working stresses up to 80 ksi."]},{"key":"dc:title","label":"Title","values":["Strength and Serviceability of Concrete Elements Reinforced with High-Strength Steel"]}]}],"canonical_facts":{"dc:contributor":["Santiago Pujol","Ayhan Irfanoglu","Julio Ramirez","Duly Abraham"],"dc:creator":["Puranam, Aishwarya Y."],"dc:date.created":["2018-05-01T07:00:00Z"],"dc:description.abstract":["The potential use of high-strength steel reinforcement (HSSR) with yield stress (𝑓𝑦) larger than 80 ksi requires reconsideration of design criteria and limits used to avoid sudden failure because they were conceived for elements with Gr. 60 and 80 (𝑓𝑦=60 and 80 ksi) reinforcement. The objective of this study is to investigate the feasibility of using HSSR for applications not related to seismic demands, with a focus on three topics: (i) minimum flexural reinforcement in slabs and walls, (ii) maximum flexural reinforcement in beams, and (iii) crack widths and deflections. Nine slabs with gross longitudinal reinforcement ratio (𝜌𝑔) between 0.07% and 0.18%, four walls with 𝜌𝑔 between 0.07% and 0.24%, and six continuous beams with longitudinal reinforcement ratio between 0.8% and 2.5% and a net tensile strain of approximately 0.005 were tested to study the strength, toughness, and serviceability of elements with HSSR. The test data indicated that it is feasible to use HSSR (with 𝑓𝑦 up to 120 ksi). The following conclusions are made in relation to the three specific topics investigated: 1) Minimum longitudinal reinforcement ratio for slabs can be reduced in inverse proportion to increase in yield stress. Test slabs with HSSR and 𝜌𝑔 as small as 0.09% had rotational capacities larger than 4%. Nevertheless prudence is due because brittle failure may occur at small displacements in lightly reinforced elements in which cracking moment approaches or exceeds yield moment and because low shear strength has been observed to be associated with low ratios of longitudinal reinforcement. 2) Current minimum longitudinal reinforcement limits in walls with uniformly distributed reinforcement, even for Gr.60 reinforcement, should be reconsidered. Specimens with Gr. 60 and Gr.120 bars, and 𝜌𝑔 ranging between 0.07% and 0.24% failed at drift capacities smaller than 1%. In walls with products of gross reinforcement ratio and measured yield stress smaller than approximately 200 psi, failure took place just after first cracking and at loads smaller than those at first cracking suggesting that elements in this range should be avoided in all structures no matter how low the probability of cracking is estimated to be. This is especially critical for ordinary structural walls without confined boundary elements in seismic regions. 3) In the tests conducted, sections with HSSR designed to have net tensile strain (𝜀𝑡) of 0.005 had sufficient rotational capacity for moment redistribution. In design, detailing to accommodate increases in shear and bond demands caused by load redistribution is needed and may be as critical as controlling maximum reinforcement ratio through 𝜀𝑡 to avoid brittle failure. 4) Test data suggest that extrapolation of minimum thickness for one-way slabs with HSSR as the thickness required for an element with working stress of 40 ksi multiplied by a factor related to working stress in the reinforcing bars (𝑓𝑠), 0.4+ 3𝑓𝑠(𝑘𝑠𝑖)200𝑘𝑠𝑖 , would lead to acceptable immediate and long-term deflections. 5) According to the measurements made, reduction in bar spacing (s) with increase in working stress in the reinforcing bars (𝑓𝑠), determined as 𝑠=15(40,000𝑓𝑠(𝑝𝑠𝑖))−2.5∗𝑐𝑜𝑣𝑒𝑟, would be sufficient to avoid intolerable crack widths even in elements with working stresses up to 80 ksi."],"dc:identifier":["https://docs.lib.purdue.edu/open_access_dissertations/1803"],"dc:title":["Strength and Serviceability of Concrete Elements Reinforced with High-Strength Steel"],"thesis:degree_discipline":["Civil Engineering"],"thesis:degree_level":["Dissertation"],"thesis:degree_name":["Doctor of Philosophy (PhD)"]},"updated_at":"2026-11-19T08:51:41Z"}