{"id":{"repo_id":"soton","oai_identifier":"oai:eprints.soton.ac.uk:464576"},"canonical_url":"https://search.ndltd.org/etd/soton/oai:eprints.soton.ac.uk:464576","repository":{"repo_id":"soton","name":"University of Southampton","base_url":"https://eprints.soton.ac.uk/cgi/oai2"},"display":{"title":"Synthesis, Structure and Electrochemistry of positive Insertion materials for rechargeable Lithium Batteries","abstract":"<p>Lithium copper oxides Li<sub>x</sub>Cu<sub>2</sub>O<sub>4</sub> (x = 2,3,4) have been synthesised for lithium battery application using solid state and solution reactions under various conditions. Li<sub>2</sub>CuO<sub>2 </sub>(I<i>mmm</i>) has been prepared in air at 800<sup>o</sup>C for 10-15 h from a stoichiometric mixture of copper oxide and lithium hydroxide. Synthesis using high pressure oxygen (250 bar, 4 h, 700<sup>o</sup>C) and hydrothermal (1.5 kbar, 10 h, 600<sup>o</sup>C) was used for the formation of mixed-valence cuprate Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub> (C2/<i>m</i>) and the isostructural Li<sub>2</sub>NaCu<sub>2 </sub>O<sub>4</sub> (250 bar in O<sub>2</sub>, 4 h, 700<sup>o</sup>C) from simple oxides. The latter has been characterised using powder neutron diffraction and crystallises in the space group C2/<i>m</i> (a = 10.2733(2), b = 2.80324 (3), c = 7.58532(9) A and β = 119.6903 (8)<sup>o</sup>). The lithium ions occupy the tetrahedral positions whereas the sodium ions are found to be exclusively in octahedral environment. LiCuO<sub>2</sub> can not be obtained directly; it was synthesised by chemical lithium extraction of the lithium rich oxide, Li<sub>3</sub>Cu<sub>3</sub>O<sub>4</sub> using Br<sub>2</sub> in CH<sub>3</sub>CN. The latter, was found to crystallise in the space group C2/<i>m</i>. The structures of all the lithium copper oxides prepared are composed of one dimensional infinite chains of edge-sharing CuO<sub>4</sub> square planes coordinated to lithium in tetrahedral (Li<sub>2</sub>CuO<sub>2</sub>, Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub>) and octahedral (LiCuO<sub>2</sub>, Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub>) positions.</p><p>Electrochemical testing was carried out in a two-electrode cell using composite electrodes containing the oxide materials, carbon black to enhance the electronic conductivity and polytetrafluoroethylene as Teflon<sup>®</sup> binder. Lithium foil has been used as reference and counter electrode and 1 M LiPF6 in EC-DMC as the electrolyte. The slow galvanostatic charging of Li<sub>2</sub>CuO<sub>2</sub> until 4.5 V yields charge specific capacity of 320 mAhg<sup>-1</sup> (theoretical capacity of 490 mAhg<sup>-1</sup>) at a cycling rate of 11 mAg<sup>-1</sup> which is followed by a large specific discharge capacity of 250 mAhg<sup>-1</sup> (0.8 Li<sup>+</sup>) distributed mostly between 2 and 3 V. Application as additive material with a positive electrode LiMn<sub>2</sub>O<sub>4</sub> was found to be successful as it compensates the initial loss of specific charge capacity due to the formation of the passivation on the negative electrode. The slow galvanostatic cycling of Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub> (theoretical capacity of 380 mAhg<sup>-1</sup>) between 1.6 and 4.5 V yields a charge density of 160 mAhg<sup>-1</sup> (0.6 Li<sup>+</sup>) at a cycling rate of 10 mAhg<sup>-1</sup>. The results for Li<sub>2</sub>NaCu<sub>2</sub>O<sub>4</sub> indicates the presence of sodium that may disrupt the lithium ion pathway. LiCuO<sub>2</sub> (theoretical capacity of 263 mAhg<sup>-1</sup>) provides between 1 and 4.3 V a specific capacity of 500 mAhg<sup>-1</sup> with an average voltage of 2.5 V. This discharge is thought to involve the formation of Cu<sup>1</sup> or Cu<sup>II</sup> in this material.</p>","abstract_html":"&lt;p&gt;Lithium copper oxides Li&lt;sub&gt;x&lt;/sub&gt;Cu&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; (x = 2,3,4) have been synthesised for lithium battery application using solid state and solution reactions under various conditions. Li&lt;sub&gt;2&lt;/sub&gt;CuO&lt;sub&gt;2 &lt;/sub&gt;(I&lt;i&gt;mmm&lt;/i&gt;) has been prepared in air at 800&lt;sup&gt;o&lt;/sup&gt;C for 10-15 h from a stoichiometric mixture of copper oxide and lithium hydroxide. Synthesis using high pressure oxygen (250 bar, 4 h, 700&lt;sup&gt;o&lt;/sup&gt;C) and hydrothermal (1.5 kbar, 10 h, 600&lt;sup&gt;o&lt;/sup&gt;C) was used for the formation of mixed-valence cuprate Li&lt;sub&gt;3&lt;/sub&gt;Cu&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; (C2/&lt;i&gt;m&lt;/i&gt;) and the isostructural Li&lt;sub&gt;2&lt;/sub&gt;NaCu&lt;sub&gt;2 &lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; (250 bar in O&lt;sub&gt;2&lt;/sub&gt;, 4 h, 700&lt;sup&gt;o&lt;/sup&gt;C) from simple oxides. The latter has been characterised using powder neutron diffraction and crystallises in the space group C2/&lt;i&gt;m&lt;/i&gt; (a = 10.2733(2), b = 2.80324 (3), c = 7.58532(9) A and β = 119.6903 (8)&lt;sup&gt;o&lt;/sup&gt;). The lithium ions occupy the tetrahedral positions whereas the sodium ions are found to be exclusively in octahedral environment. LiCuO&lt;sub&gt;2&lt;/sub&gt; can not be obtained directly; it was synthesised by chemical lithium extraction of the lithium rich oxide, Li&lt;sub&gt;3&lt;/sub&gt;Cu&lt;sub&gt;3&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; using Br&lt;sub&gt;2&lt;/sub&gt; in CH&lt;sub&gt;3&lt;/sub&gt;CN. The latter, was found to crystallise in the space group C2/&lt;i&gt;m&lt;/i&gt;. The structures of all the lithium copper oxides prepared are composed of one dimensional infinite chains of edge-sharing CuO&lt;sub&gt;4&lt;/sub&gt; square planes coordinated to lithium in tetrahedral (Li&lt;sub&gt;2&lt;/sub&gt;CuO&lt;sub&gt;2&lt;/sub&gt;, Li&lt;sub&gt;3&lt;/sub&gt;Cu&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt;) and octahedral (LiCuO&lt;sub&gt;2&lt;/sub&gt;, Li&lt;sub&gt;3&lt;/sub&gt;Cu&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt;) positions.&lt;/p&gt;&lt;p&gt;Electrochemical testing was carried out in a two-electrode cell using composite electrodes containing the oxide materials, carbon black to enhance the electronic conductivity and polytetrafluoroethylene as Teflon&lt;sup&gt;®&lt;/sup&gt; binder. Lithium foil has been used as reference and counter electrode and 1 M LiPF6 in EC-DMC as the electrolyte. The slow galvanostatic charging of Li&lt;sub&gt;2&lt;/sub&gt;CuO&lt;sub&gt;2&lt;/sub&gt; until 4.5 V yields charge specific capacity of 320 mAhg&lt;sup&gt;-1&lt;/sup&gt; (theoretical capacity of 490 mAhg&lt;sup&gt;-1&lt;/sup&gt;) at a cycling rate of 11 mAg&lt;sup&gt;-1&lt;/sup&gt; which is followed by a large specific discharge capacity of 250 mAhg&lt;sup&gt;-1&lt;/sup&gt; (0.8 Li&lt;sup&gt;+&lt;/sup&gt;) distributed mostly between 2 and 3 V. Application as additive material with a positive electrode LiMn&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; was found to be successful as it compensates the initial loss of specific charge capacity due to the formation of the passivation on the negative electrode. The slow galvanostatic cycling of Li&lt;sub&gt;3&lt;/sub&gt;Cu&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; (theoretical capacity of 380 mAhg&lt;sup&gt;-1&lt;/sup&gt;) between 1.6 and 4.5 V yields a charge density of 160 mAhg&lt;sup&gt;-1&lt;/sup&gt; (0.6 Li&lt;sup&gt;+&lt;/sup&gt;) at a cycling rate of 10 mAhg&lt;sup&gt;-1&lt;/sup&gt;. The results for Li&lt;sub&gt;2&lt;/sub&gt;NaCu&lt;sub&gt;2&lt;/sub&gt;O&lt;sub&gt;4&lt;/sub&gt; indicates the presence of sodium that may disrupt the lithium ion pathway. LiCuO&lt;sub&gt;2&lt;/sub&gt; (theoretical capacity of 263 mAhg&lt;sup&gt;-1&lt;/sup&gt;) provides between 1 and 4.3 V a specific capacity of 500 mAhg&lt;sup&gt;-1&lt;/sup&gt; with an average voltage of 2.5 V. This discharge is thought to involve the formation of Cu&lt;sup&gt;1&lt;/sup&gt; or Cu&lt;sup&gt;II&lt;/sup&gt; in this material.&lt;/p&gt;","abstract_has_math":false,"creators":["Raekelboom, Emmanuelle Angeline"],"institution":"University of Southampton","degree_name":"Ph.D.","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2002,"date_issued":"2002","date_published":"2002","updated_at":"2026-11-19T09:36:57Z","subjects":[],"languages":["English","eng"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://eprints.soton.ac.uk/id/eprint/464576/1/834701.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://eprints.soton.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aeprints.soton.ac.uk%3A464576","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:creator","label":"Author","values":["Raekelboom, Emmanuelle Angeline"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2002"]},{"key":"dc:date.issued","label":"Date","values":["2002"]},{"key":"dc:publisher.commercial","label":"Dc Publisher Commercial","values":["University of Southampton"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Chemistry (pre 2011 reorg)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Southampton"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://eprints.soton.ac.uk/id/eprint/464576/"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D."]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["English"]},{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://eprints.soton.ac.uk/id/eprint/464576/1/834701.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["<p>Lithium copper oxides Li<sub>x</sub>Cu<sub>2</sub>O<sub>4</sub> (x = 2,3,4) have been synthesised for lithium battery application using solid state and solution reactions under various conditions. Li<sub>2</sub>CuO<sub>2 </sub>(I<i>mmm</i>) has been prepared in air at 800<sup>o</sup>C for 10-15 h from a stoichiometric mixture of copper oxide and lithium hydroxide. Synthesis using high pressure oxygen (250 bar, 4 h, 700<sup>o</sup>C) and hydrothermal (1.5 kbar, 10 h, 600<sup>o</sup>C) was used for the formation of mixed-valence cuprate Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub> (C2/<i>m</i>) and the isostructural Li<sub>2</sub>NaCu<sub>2 </sub>O<sub>4</sub> (250 bar in O<sub>2</sub>, 4 h, 700<sup>o</sup>C) from simple oxides. The latter has been characterised using powder neutron diffraction and crystallises in the space group C2/<i>m</i> (a = 10.2733(2), b = 2.80324 (3), c = 7.58532(9) A and β = 119.6903 (8)<sup>o</sup>). The lithium ions occupy the tetrahedral positions whereas the sodium ions are found to be exclusively in octahedral environment. LiCuO<sub>2</sub> can not be obtained directly; it was synthesised by chemical lithium extraction of the lithium rich oxide, Li<sub>3</sub>Cu<sub>3</sub>O<sub>4</sub> using Br<sub>2</sub> in CH<sub>3</sub>CN. The latter, was found to crystallise in the space group C2/<i>m</i>. The structures of all the lithium copper oxides prepared are composed of one dimensional infinite chains of edge-sharing CuO<sub>4</sub> square planes coordinated to lithium in tetrahedral (Li<sub>2</sub>CuO<sub>2</sub>, Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub>) and octahedral (LiCuO<sub>2</sub>, Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub>) positions.</p><p>Electrochemical testing was carried out in a two-electrode cell using composite electrodes containing the oxide materials, carbon black to enhance the electronic conductivity and polytetrafluoroethylene as Teflon<sup>®</sup> binder. Lithium foil has been used as reference and counter electrode and 1 M LiPF6 in EC-DMC as the electrolyte. The slow galvanostatic charging of Li<sub>2</sub>CuO<sub>2</sub> until 4.5 V yields charge specific capacity of 320 mAhg<sup>-1</sup> (theoretical capacity of 490 mAhg<sup>-1</sup>) at a cycling rate of 11 mAg<sup>-1</sup> which is followed by a large specific discharge capacity of 250 mAhg<sup>-1</sup> (0.8 Li<sup>+</sup>) distributed mostly between 2 and 3 V. Application as additive material with a positive electrode LiMn<sub>2</sub>O<sub>4</sub> was found to be successful as it compensates the initial loss of specific charge capacity due to the formation of the passivation on the negative electrode. The slow galvanostatic cycling of Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub> (theoretical capacity of 380 mAhg<sup>-1</sup>) between 1.6 and 4.5 V yields a charge density of 160 mAhg<sup>-1</sup> (0.6 Li<sup>+</sup>) at a cycling rate of 10 mAhg<sup>-1</sup>. The results for Li<sub>2</sub>NaCu<sub>2</sub>O<sub>4</sub> indicates the presence of sodium that may disrupt the lithium ion pathway. LiCuO<sub>2</sub> (theoretical capacity of 263 mAhg<sup>-1</sup>) provides between 1 and 4.3 V a specific capacity of 500 mAhg<sup>-1</sup> with an average voltage of 2.5 V. This discharge is thought to involve the formation of Cu<sup>1</sup> or Cu<sup>II</sup> in this material.</p>"]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Synthesis, Structure and Electrochemistry of positive Insertion materials for rechargeable Lithium Batteries"]}]}],"canonical_facts":{"dc:creator":["Raekelboom, Emmanuelle Angeline"],"dc:date":["2002"],"dc:date.issued":["2002"],"dc:description.abstract":["<p>Lithium copper oxides Li<sub>x</sub>Cu<sub>2</sub>O<sub>4</sub> (x = 2,3,4) have been synthesised for lithium battery application using solid state and solution reactions under various conditions. Li<sub>2</sub>CuO<sub>2 </sub>(I<i>mmm</i>) has been prepared in air at 800<sup>o</sup>C for 10-15 h from a stoichiometric mixture of copper oxide and lithium hydroxide. Synthesis using high pressure oxygen (250 bar, 4 h, 700<sup>o</sup>C) and hydrothermal (1.5 kbar, 10 h, 600<sup>o</sup>C) was used for the formation of mixed-valence cuprate Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub> (C2/<i>m</i>) and the isostructural Li<sub>2</sub>NaCu<sub>2 </sub>O<sub>4</sub> (250 bar in O<sub>2</sub>, 4 h, 700<sup>o</sup>C) from simple oxides. The latter has been characterised using powder neutron diffraction and crystallises in the space group C2/<i>m</i> (a = 10.2733(2), b = 2.80324 (3), c = 7.58532(9) A and β = 119.6903 (8)<sup>o</sup>). The lithium ions occupy the tetrahedral positions whereas the sodium ions are found to be exclusively in octahedral environment. LiCuO<sub>2</sub> can not be obtained directly; it was synthesised by chemical lithium extraction of the lithium rich oxide, Li<sub>3</sub>Cu<sub>3</sub>O<sub>4</sub> using Br<sub>2</sub> in CH<sub>3</sub>CN. The latter, was found to crystallise in the space group C2/<i>m</i>. The structures of all the lithium copper oxides prepared are composed of one dimensional infinite chains of edge-sharing CuO<sub>4</sub> square planes coordinated to lithium in tetrahedral (Li<sub>2</sub>CuO<sub>2</sub>, Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub>) and octahedral (LiCuO<sub>2</sub>, Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub>) positions.</p><p>Electrochemical testing was carried out in a two-electrode cell using composite electrodes containing the oxide materials, carbon black to enhance the electronic conductivity and polytetrafluoroethylene as Teflon<sup>®</sup> binder. Lithium foil has been used as reference and counter electrode and 1 M LiPF6 in EC-DMC as the electrolyte. The slow galvanostatic charging of Li<sub>2</sub>CuO<sub>2</sub> until 4.5 V yields charge specific capacity of 320 mAhg<sup>-1</sup> (theoretical capacity of 490 mAhg<sup>-1</sup>) at a cycling rate of 11 mAg<sup>-1</sup> which is followed by a large specific discharge capacity of 250 mAhg<sup>-1</sup> (0.8 Li<sup>+</sup>) distributed mostly between 2 and 3 V. Application as additive material with a positive electrode LiMn<sub>2</sub>O<sub>4</sub> was found to be successful as it compensates the initial loss of specific charge capacity due to the formation of the passivation on the negative electrode. The slow galvanostatic cycling of Li<sub>3</sub>Cu<sub>2</sub>O<sub>4</sub> (theoretical capacity of 380 mAhg<sup>-1</sup>) between 1.6 and 4.5 V yields a charge density of 160 mAhg<sup>-1</sup> (0.6 Li<sup>+</sup>) at a cycling rate of 10 mAhg<sup>-1</sup>. The results for Li<sub>2</sub>NaCu<sub>2</sub>O<sub>4</sub> indicates the presence of sodium that may disrupt the lithium ion pathway. LiCuO<sub>2</sub> (theoretical capacity of 263 mAhg<sup>-1</sup>) provides between 1 and 4.3 V a specific capacity of 500 mAhg<sup>-1</sup> with an average voltage of 2.5 V. This discharge is thought to involve the formation of Cu<sup>1</sup> or Cu<sup>II</sup> in this material.</p>"],"dc:format":["text"],"dc:identifier.uri":["https://eprints.soton.ac.uk/id/eprint/464576/1/834701.pdf"],"dc:language":["English"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.commercial":["University of Southampton"],"dc:publisher.department":["Chemistry (pre 2011 reorg)"],"dc:publisher.institution":["University of Southampton"],"dc:relation.isreferencedby":["https://eprints.soton.ac.uk/id/eprint/464576/"],"dcterms:accessrights":["public"],"dc:title":["Synthesis, Structure and Electrochemistry of positive Insertion materials for rechargeable Lithium Batteries"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D."]},"updated_at":"2026-11-19T09:36:57Z"}