{"id":{"repo_id":"texas-state","oai_identifier":"oai:digital.library.txst.edu:10877/22983"},"canonical_url":"https://search.ndltd.org/etd/texas-state/oai:digital.library.txst.edu:10877/22983","repository":{"repo_id":"texas-state","name":"Texas State University","base_url":"https://digital.library.txst.edu/server/oai/request"},"display":{"title":"Advancing Diamond Growth Techniques: Investigating the Impact of Multi-Stage Methane Concentration on Diamond Growth using HFCVD","abstract":"This dissertation presents a comparative study of polycrystalline diamond films grown using a two-step methane concentration approach in hot filament chemical vapor deposition (HFCVD), with the goal of achieving high-quality films in shorter growth times. The research investigates how the sequencing of methane concentrations affects the coalescence of diamond seeds, total growth rate and final diamond quality. Previous study shows that using a higher methane concentration increases the growth rate as well as non-diamond carbon (NDC) content due to the availability of more methyl radicals. And using low methane concentration (1.5% or 1.0%) results in enhanced quality (low NDC content) diamonds due to more H-etching than higher methane concentration growth. However, doing so requires longer growth time due to the availability of less methyl radical. Consequently, processes within the HFCVD framework are needed to minimize the growth rate while keeping the diamond quality comparable to lower-concentration methane growth. This dissertation presents a detailed study on the growth and characterization of polycrystalline diamond films using a two-step methane concentration growth in HFCVD. The goal was to balance growth rate and film quality by combining the advantages of both high and low methane concentration during the growth. Multiple samples were grown using both two-step and single-step methane concentration growth using methane concentration varying from 1.0%-3.0%. The two-step growths included sequences with high-to-low and low-to-high methane concentrations, while the single-step processes used either high or low methane concentration throughout the growth. The samples morphology was thoroughly characterized using atomic force microscopy (AFM), scanning electron microscopy (SEM), high-resolution scanning transmission electron microscopy (HRSTEM), X-ray diffraction (XRD) and diamond quality was assessed using in-built UV-Raman spectroscopy. Two different approaches were used to study diamond films using a two-step methane concentration growth. In the first approach, growth was initiated with a low methane concentration followed by a transition to a higher concentration. In the second approach, a high methane concentration was used in the initial phase, followed by a lower concentration in the subsequent phase. For similar thickness samples, comparative analysis of these methods revealed that initiating growth with low methane concentration resulted in lower-quality diamond films, as indicated by a reduced Raman peak intensity ratio and full width half maxima (ΔFWHM) values (~0.31 and 4.1 cm⁻¹, respectively). In contrast, the high-to-low methane growth produced better film quality, with a higher Raman peak ratio (~0.48) and narrower ΔFWHM (~3.9 cm⁻¹). This improvement is attributed to the fact that higher methane concentration in the initial phase promotes faster coalescence of diamond seeds, while the subsequent lower methane phase provides a hydrogen-rich environment that enhances the etching of non-diamond carbon (NDC). Thus, the high-to-low methane transition proved to be a more effective strategy for producing high-quality diamond films. Another significant outcome of the two-step methane concentration growth is its ability to achieve comparable diamond film quality in a significantly shorter growth duration compared to conventional single step lower methane concentration growth. For instance, the two-step growth using 3.0%-1h+1.5%-3h, yielded a Raman peak ratio and ΔFWHM of ~0.68 and 3.40 cm⁻¹, respectively. These values are comparable to those obtained from, single-step growth using 1.5%-7h, which showed a peak ratio and ΔFWHM of ~0.68 and 2.96 cm⁻¹. This indicates that the two-step approach can produce similar crystalline quality while reducing the total deposition time by nearly 40%. Overall, this research validates an efficient two-step methane growth method for producing high-quality polycrystalline diamond films with fewer defects, better morphology at reduced growth time. These findings offer a promising pathway toward integrating diamond into next-generation high-power electronics and thermal spreaders.","abstract_html":"This dissertation presents a comparative study of polycrystalline diamond films grown using a two-step methane concentration approach in hot filament chemical vapor deposition (HFCVD), with the goal of achieving high-quality films in shorter growth times. The research investigates how the sequencing of methane concentrations affects the coalescence of diamond seeds, total growth rate and final diamond quality. Previous study shows that using a higher methane concentration increases the growth rate as well as non-diamond carbon (NDC) content due to the availability of more methyl radicals. And using low methane concentration (1.5% or 1.0%) results in enhanced quality (low NDC content) diamonds due to more H-etching than higher methane concentration growth. However, doing so requires longer growth time due to the availability of less methyl radical. Consequently, processes within the HFCVD framework are needed to minimize the growth rate while keeping the diamond quality comparable to lower-concentration methane growth. This dissertation presents a detailed study on the growth and characterization of polycrystalline diamond films using a two-step methane concentration growth in HFCVD. The goal was to balance growth rate and film quality by combining the advantages of both high and low methane concentration during the growth. Multiple samples were grown using both two-step and single-step methane concentration growth using methane concentration varying from 1.0%-3.0%. The two-step growths included sequences with high-to-low and low-to-high methane concentrations, while the single-step processes used either high or low methane concentration throughout the growth. The samples morphology was thoroughly characterized using atomic force microscopy (AFM), scanning electron microscopy (SEM), high-resolution scanning transmission electron microscopy (HRSTEM), X-ray diffraction (XRD) and diamond quality was assessed using in-built UV-Raman spectroscopy. Two different approaches were used to study diamond films using a two-step methane concentration growth. In the first approach, growth was initiated with a low methane concentration followed by a transition to a higher concentration. In the second approach, a high methane concentration was used in the initial phase, followed by a lower concentration in the subsequent phase. For similar thickness samples, comparative analysis of these methods revealed that initiating growth with low methane concentration resulted in lower-quality diamond films, as indicated by a reduced Raman peak intensity ratio and full width half maxima (ΔFWHM) values (~0.31 and 4.1 cm⁻¹, respectively). In contrast, the high-to-low methane growth produced better film quality, with a higher Raman peak ratio (~0.48) and narrower ΔFWHM (~3.9 cm⁻¹). This improvement is attributed to the fact that higher methane concentration in the initial phase promotes faster coalescence of diamond seeds, while the subsequent lower methane phase provides a hydrogen-rich environment that enhances the etching of non-diamond carbon (NDC). Thus, the high-to-low methane transition proved to be a more effective strategy for producing high-quality diamond films. Another significant outcome of the two-step methane concentration growth is its ability to achieve comparable diamond film quality in a significantly shorter growth duration compared to conventional single step lower methane concentration growth. For instance, the two-step growth using 3.0%-1h+1.5%-3h, yielded a Raman peak ratio and ΔFWHM of ~0.68 and 3.40 cm⁻¹, respectively. These values are comparable to those obtained from, single-step growth using 1.5%-7h, which showed a peak ratio and ΔFWHM of ~0.68 and 2.96 cm⁻¹. This indicates that the two-step approach can produce similar crystalline quality while reducing the total deposition time by nearly 40%. Overall, this research validates an efficient two-step methane growth method for producing high-quality polycrystalline diamond films with fewer defects, better morphology at reduced growth time. These findings offer a promising pathway toward integrating diamond into next-generation high-power electronics and thermal spreaders.","abstract_has_math":false,"creators":["Devkota, Dipa"],"institution":"Texas State University","degree_name":"Doctor of Philosophy","degree_level":"Doctoral","degree_discipline":"Materials Science, Engineering, and Commercialization","degree_department":"Materials Science, Engineering, and Commercialization","school":null,"contributors":[],"advisors":["Piner, Edwin L.","Holtz, Mark W."],"committee_chairs":[],"committee_members":["Haque, Ariful","Engdhal, Chris","Geerts, Wilhelmus"],"year":2025,"date_issued":"2025-08","date_published":"2025-08","updated_at":"2026-11-20T16:08:07Z","subjects":["diamond","high power electronics","HFCVD"],"languages":["en"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier.citation","label":"Dc Identifier Citation","values":["Devkota, D. (2025). Advancing diamond growth techniques: Investigating the impact of multi-stage methane concentration on diamond growth using HFCVD. [Doctoral dissertation, Texas State University]."],"render_values":[{"text":"Devkota, D. (2025). Advancing diamond growth techniques: Investigating the impact of multi-stage methane concentration on diamond growth using HFCVD. [Doctoral dissertation, Texas State University].","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":"https://hdl.handle.net/10877/22983","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"https://hdl.handle.net/10877/22983","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Atexas-state%3Aoai%3Adigital.library.txst.edu%3A10877%2F22983","prefix":"oai_dc"},"source_record":{"url":"https://digital.library.txst.edu/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Adigital.library.txst.edu%3A10877%2F22983","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Piner, Edwin L.","Holtz, Mark W."]},{"key":"dc:contributor.committeemember","label":"Committee Member","values":["Haque, Ariful","Engdhal, Chris","Geerts, Wilhelmus"]},{"key":"dc:contributor.department","label":"Department","values":["Materials Science, Engineering, and Commercialization"]},{"key":"dc:creator","label":"Author","values":["Devkota, Dipa"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2025-10-10T17:14:13Z"]},{"key":"dc:date.issued","label":"Date","values":["2025-08"]},{"key":"dc:type","label":"Dc Type","values":["Dissertation"]},{"key":"thesis:degree_department","label":"Department","values":["Materials Science, Engineering, and Commercialization"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Materials Science, Engineering, and Commercialization"]},{"key":"thesis:degree_level","label":"Degree Level","values":["Doctoral"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Doctor of Philosophy"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["Texas State University"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["diamond","high power electronics","HFCVD"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.iso","label":"Language (ISO)","values":["en"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.citation","label":"Dc Identifier Citation","values":["Devkota, D. (2025). Advancing diamond growth techniques: Investigating the impact of multi-stage methane concentration on diamond growth using HFCVD. [Doctoral dissertation, Texas State University]."]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://hdl.handle.net/10877/22983"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["This dissertation presents a comparative study of polycrystalline diamond films grown using a two-step methane concentration approach in hot filament chemical vapor deposition (HFCVD), with the goal of achieving high-quality films in shorter growth times. The research investigates how the sequencing of methane concentrations affects the coalescence of diamond seeds, total growth rate and final diamond quality. Previous study shows that using a higher methane concentration increases the growth rate as well as non-diamond carbon (NDC) content due to the availability of more methyl radicals. And using low methane concentration (1.5% or 1.0%) results in enhanced quality (low NDC content) diamonds due to more H-etching than higher methane concentration growth. However, doing so requires longer growth time due to the availability of less methyl radical. Consequently, processes within the HFCVD framework are needed to minimize the growth rate while keeping the diamond quality comparable to lower-concentration methane growth. This dissertation presents a detailed study on the growth and characterization of polycrystalline diamond films using a two-step methane concentration growth in HFCVD. The goal was to balance growth rate and film quality by combining the advantages of both high and low methane concentration during the growth. Multiple samples were grown using both two-step and single-step methane concentration growth using methane concentration varying from 1.0%-3.0%. The two-step growths included sequences with high-to-low and low-to-high methane concentrations, while the single-step processes used either high or low methane concentration throughout the growth. The samples morphology was thoroughly characterized using atomic force microscopy (AFM), scanning electron microscopy (SEM), high-resolution scanning transmission electron microscopy (HRSTEM), X-ray diffraction (XRD) and diamond quality was assessed using in-built UV-Raman spectroscopy. Two different approaches were used to study diamond films using a two-step methane concentration growth. In the first approach, growth was initiated with a low methane concentration followed by a transition to a higher concentration. In the second approach, a high methane concentration was used in the initial phase, followed by a lower concentration in the subsequent phase. For similar thickness samples, comparative analysis of these methods revealed that initiating growth with low methane concentration resulted in lower-quality diamond films, as indicated by a reduced Raman peak intensity ratio and full width half maxima (ΔFWHM) values (~0.31 and 4.1 cm⁻¹, respectively). In contrast, the high-to-low methane growth produced better film quality, with a higher Raman peak ratio (~0.48) and narrower ΔFWHM (~3.9 cm⁻¹). This improvement is attributed to the fact that higher methane concentration in the initial phase promotes faster coalescence of diamond seeds, while the subsequent lower methane phase provides a hydrogen-rich environment that enhances the etching of non-diamond carbon (NDC). Thus, the high-to-low methane transition proved to be a more effective strategy for producing high-quality diamond films. Another significant outcome of the two-step methane concentration growth is its ability to achieve comparable diamond film quality in a significantly shorter growth duration compared to conventional single step lower methane concentration growth. For instance, the two-step growth using 3.0%-1h+1.5%-3h, yielded a Raman peak ratio and ΔFWHM of ~0.68 and 3.40 cm⁻¹, respectively. These values are comparable to those obtained from, single-step growth using 1.5%-7h, which showed a peak ratio and ΔFWHM of ~0.68 and 2.96 cm⁻¹. This indicates that the two-step approach can produce similar crystalline quality while reducing the total deposition time by nearly 40%. Overall, this research validates an efficient two-step methane growth method for producing high-quality polycrystalline diamond films with fewer defects, better morphology at reduced growth time. These findings offer a promising pathway toward integrating diamond into next-generation high-power electronics and thermal spreaders."]},{"key":"dc:format","label":"Dc Format","values":["Text"]},{"key":"dc:format.extent","label":"Dc Format Extent","values":["174 pages"]},{"key":"dc:format.medium","label":"Dc Format Medium","values":["1 file (.pdf)"]},{"key":"dc:title","label":"Title","values":["Advancing Diamond Growth Techniques: Investigating the Impact of Multi-Stage Methane Concentration on Diamond Growth using HFCVD"]},{"key":"others:access_status","label":"Others Access Status","values":["open.access"]}]}],"canonical_facts":{"dc:contributor.advisor":["Piner, Edwin L.","Holtz, Mark W."],"dc:contributor.committeemember":["Haque, Ariful","Engdhal, Chris","Geerts, Wilhelmus"],"dc:contributor.department":["Materials Science, Engineering, and Commercialization"],"dc:creator":["Devkota, Dipa"],"dc:date.accessioned":["2025-10-10T17:14:13Z"],"dc:date.issued":["2025-08"],"dc:description.abstract":["This dissertation presents a comparative study of polycrystalline diamond films grown using a two-step methane concentration approach in hot filament chemical vapor deposition (HFCVD), with the goal of achieving high-quality films in shorter growth times. The research investigates how the sequencing of methane concentrations affects the coalescence of diamond seeds, total growth rate and final diamond quality. Previous study shows that using a higher methane concentration increases the growth rate as well as non-diamond carbon (NDC) content due to the availability of more methyl radicals. And using low methane concentration (1.5% or 1.0%) results in enhanced quality (low NDC content) diamonds due to more H-etching than higher methane concentration growth. However, doing so requires longer growth time due to the availability of less methyl radical. Consequently, processes within the HFCVD framework are needed to minimize the growth rate while keeping the diamond quality comparable to lower-concentration methane growth. This dissertation presents a detailed study on the growth and characterization of polycrystalline diamond films using a two-step methane concentration growth in HFCVD. The goal was to balance growth rate and film quality by combining the advantages of both high and low methane concentration during the growth. Multiple samples were grown using both two-step and single-step methane concentration growth using methane concentration varying from 1.0%-3.0%. The two-step growths included sequences with high-to-low and low-to-high methane concentrations, while the single-step processes used either high or low methane concentration throughout the growth. The samples morphology was thoroughly characterized using atomic force microscopy (AFM), scanning electron microscopy (SEM), high-resolution scanning transmission electron microscopy (HRSTEM), X-ray diffraction (XRD) and diamond quality was assessed using in-built UV-Raman spectroscopy. Two different approaches were used to study diamond films using a two-step methane concentration growth. In the first approach, growth was initiated with a low methane concentration followed by a transition to a higher concentration. In the second approach, a high methane concentration was used in the initial phase, followed by a lower concentration in the subsequent phase. For similar thickness samples, comparative analysis of these methods revealed that initiating growth with low methane concentration resulted in lower-quality diamond films, as indicated by a reduced Raman peak intensity ratio and full width half maxima (ΔFWHM) values (~0.31 and 4.1 cm⁻¹, respectively). In contrast, the high-to-low methane growth produced better film quality, with a higher Raman peak ratio (~0.48) and narrower ΔFWHM (~3.9 cm⁻¹). This improvement is attributed to the fact that higher methane concentration in the initial phase promotes faster coalescence of diamond seeds, while the subsequent lower methane phase provides a hydrogen-rich environment that enhances the etching of non-diamond carbon (NDC). Thus, the high-to-low methane transition proved to be a more effective strategy for producing high-quality diamond films. Another significant outcome of the two-step methane concentration growth is its ability to achieve comparable diamond film quality in a significantly shorter growth duration compared to conventional single step lower methane concentration growth. For instance, the two-step growth using 3.0%-1h+1.5%-3h, yielded a Raman peak ratio and ΔFWHM of ~0.68 and 3.40 cm⁻¹, respectively. These values are comparable to those obtained from, single-step growth using 1.5%-7h, which showed a peak ratio and ΔFWHM of ~0.68 and 2.96 cm⁻¹. This indicates that the two-step approach can produce similar crystalline quality while reducing the total deposition time by nearly 40%. Overall, this research validates an efficient two-step methane growth method for producing high-quality polycrystalline diamond films with fewer defects, better morphology at reduced growth time. These findings offer a promising pathway toward integrating diamond into next-generation high-power electronics and thermal spreaders."],"dc:format":["Text"],"dc:format.extent":["174 pages"],"dc:format.medium":["1 file (.pdf)"],"dc:identifier.citation":["Devkota, D. (2025). Advancing diamond growth techniques: Investigating the impact of multi-stage methane concentration on diamond growth using HFCVD. [Doctoral dissertation, Texas State University]."],"dc:identifier.uri":["https://hdl.handle.net/10877/22983"],"dc:language.iso":["en"],"dc:subject":["diamond","high power electronics","HFCVD"],"dc:title":["Advancing Diamond Growth Techniques: Investigating the Impact of Multi-Stage Methane Concentration on Diamond Growth using HFCVD"],"dc:type":["Dissertation"],"others:access_status":["open.access"],"thesis:degree_department":["Materials Science, Engineering, and Commercialization"],"thesis:degree_discipline":["Materials Science, Engineering, and Commercialization"],"thesis:degree_level":["Doctoral"],"thesis:degree_name":["Doctor of Philosophy"],"thesis:institution_name":["Texas State University"]},"updated_at":"2026-11-20T16:08:07Z"}