{"id":{"repo_id":"uab","oai_identifier":"oai:digitalcommons.library.uab.edu:etd-collection-3081"},"canonical_url":"https://search.ndltd.org/etd/uab/oai:digitalcommons.library.uab.edu:etd-collection-3081","repository":{"repo_id":"uab","name":"University of Alabama Birmingham","base_url":"https://digitalcommons.library.uab.edu/do/oai/"},"display":{"title":"Fracture Strength of Translucent Zirconia Crowns","abstract":"ABSTRACT Objectives: To measure and compare crown fracture load of a new translucent zirconia. Methods: 72 Standarized crown preparations were designed with AutoCAD software with a 0.8mm shoulder margin and 1 mm incisal-cervical marginal curvature. A stylized crown with a 1mm thickness and 0.8mm minimum thickness in the central pit was designed in 3shape software. Tooth dies were milled out of a resin composite (Crystal Ultra) that has a similar modulus as dentin (Modulus 10 GPa). Crowns were fabricated and prepared into the following groups: 24 crowns of translucent zirconia (Lava Esthetic, 3M), 8 bonded with resin cement (Group 1), 8 alumina particle abraded bonded with a resin cement (Group 4) and 8 cemented with resin-modified glass ionomer (Group 7); 24 crowns out of traditional zirconia (Lava Plus, 3M) 8 bonded with resin cement (Group 2), 8 alumina particle abraded bonded with a resin cement (Group 5) and 8 cemented with resin-modified glass ionomer (Group 8); 24 crowns out of lithium disilicate (e.max CAD, Ivoclar Vivadent), 8 bonded with resin cement (Group 3), 8 etched with 5% hydrofluoric acid and silane application bonded with a resin cement (Group 6) and 8 cemented with resin-modified glass ionomer (Group 9). All the crowns were load cycled for 100,000 cycles at 100 N force in a custom fatigue device. Specimens were loaded against a stainless steel ball that made contact with the stylized crowns on each of the four cusps. All fatiguing was performed in 24 C water. The crowns were then fractured in a universal testing machine (MTS). The load was applied with a stainless steel indenter (7mm radius) with a loading rate of 1 mm/min. A 1.5mm rubber sheet was placed between the indenter and the crown to be distributed the load and simulate a food bolus. Results: Lava Plus bonded with self-adhesive resin cement (Group 2) showed the highest values 5383.5 +/- 713.0, followed by Lava Plus with sandblast treatment and bonded with a self-adhesive resin cement (Group 5) 5272.2 +/- 383.2. The lowest value was shown by Lava Esthetic cemented with a RMGI (Group 7) 3007.4 +/- 320.8c. The crowns milled out of e.max CAD (Group 9) failed the during the load cycle test. Conclusions: The strength of Lava Esthetic and e.max CAD are about 2/3 that of Lava Plus when bonded with a resin cement. All materials are strengthened when bonded with a resin cement. When bonded with a resin cement, Lava Esthetic is not weakened with sandblasting. When cemented with a RMGI cement, Lava Esthetic shows a lower fatigue resistance when sandblasted than when sandblasting is omitted. When cemented with a RMGI cement, Lava Esthetic showed a better fatigue resistance than e.max CAD.","abstract_html":"ABSTRACT Objectives: To measure and compare crown fracture load of a new translucent zirconia. Methods: 72 Standarized crown preparations were designed with AutoCAD software with a 0.8mm shoulder margin and 1 mm incisal-cervical marginal curvature. A stylized crown with a 1mm thickness and 0.8mm minimum thickness in the central pit was designed in 3shape software. Tooth dies were milled out of a resin composite (Crystal Ultra) that has a similar modulus as dentin (Modulus 10 GPa). Crowns were fabricated and prepared into the following groups: 24 crowns of translucent zirconia (Lava Esthetic, 3M), 8 bonded with resin cement (Group 1), 8 alumina particle abraded bonded with a resin cement (Group 4) and 8 cemented with resin-modified glass ionomer (Group 7); 24 crowns out of traditional zirconia (Lava Plus, 3M) 8 bonded with resin cement (Group 2), 8 alumina particle abraded bonded with a resin cement (Group 5) and 8 cemented with resin-modified glass ionomer (Group 8); 24 crowns out of lithium disilicate (e.max CAD, Ivoclar Vivadent), 8 bonded with resin cement (Group 3), 8 etched with 5% hydrofluoric acid and silane application bonded with a resin cement (Group 6) and 8 cemented with resin-modified glass ionomer (Group 9). All the crowns were load cycled for 100,000 cycles at 100 N force in a custom fatigue device. Specimens were loaded against a stainless steel ball that made contact with the stylized crowns on each of the four cusps. All fatiguing was performed in 24 C water. The crowns were then fractured in a universal testing machine (MTS). The load was applied with a stainless steel indenter (7mm radius) with a loading rate of 1 mm/min. A 1.5mm rubber sheet was placed between the indenter and the crown to be distributed the load and simulate a food bolus. Results: Lava Plus bonded with self-adhesive resin cement (Group 2) showed the highest values 5383.5 +/- 713.0, followed by Lava Plus with sandblast treatment and bonded with a self-adhesive resin cement (Group 5) 5272.2 +/- 383.2. The lowest value was shown by Lava Esthetic cemented with a RMGI (Group 7) 3007.4 +/- 320.8c. The crowns milled out of e.max CAD (Group 9) failed the during the load cycle test. Conclusions: The strength of Lava Esthetic and e.max CAD are about 2/3 that of Lava Plus when bonded with a resin cement. All materials are strengthened when bonded with a resin cement. When bonded with a resin cement, Lava Esthetic is not weakened with sandblasting. When cemented with a RMGI cement, Lava Esthetic shows a lower fatigue resistance when sandblasted than when sandblasting is omitted. When cemented with a RMGI cement, Lava Esthetic showed a better fatigue resistance than e.max CAD.","abstract_has_math":false,"creators":["Jurado, Carlos Alberto"],"institution":null,"degree_name":null,"degree_level":"Thesis","degree_discipline":null,"degree_department":null,"school":null,"contributors":["Nathaniel Lawson","Daniel Givan","Perng-Ru Liu","Keith Kinderknecht"],"advisors":[],"committee_chairs":[],"committee_members":[],"year":null,"date_issued":"","date_published":null,"updated_at":"2026-11-19T09:26:30Z","subjects":["Dentistry"],"languages":[],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"https://digitalcommons.library.uab.edu/etd-collection/2089","outbound_label":"Repository record","outbound_source":"dc:identifier","record_url":"https://digitalcommons.library.uab.edu/etd-collection/2089","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier","download_url":null,"download_label":null,"download_source":null,"access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://digitalcommons.library.uab.edu/do/oai/?verb=GetRecord&metadataPrefix=oai_etdms&identifier=oai%3Adigitalcommons.library.uab.edu%3Aetd-collection-3081","prefix":"oai_etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor","label":"Contributor","values":["Nathaniel Lawson","Daniel Givan","Perng-Ru Liu","Keith Kinderknecht"]},{"key":"dc:creator","label":"Author","values":["Jurado, Carlos Alberto"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.created","label":"Dc Date Created","values":["2018-01-01T08:00:00Z"]},{"key":"thesis:degree_level","label":"Degree Level","values":["Thesis"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Dentistry"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["https://digitalcommons.library.uab.edu/etd-collection/2089"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["ABSTRACT Objectives: To measure and compare crown fracture load of a new translucent zirconia. Methods: 72 Standarized crown preparations were designed with AutoCAD software with a 0.8mm shoulder margin and 1 mm incisal-cervical marginal curvature. A stylized crown with a 1mm thickness and 0.8mm minimum thickness in the central pit was designed in 3shape software. Tooth dies were milled out of a resin composite (Crystal Ultra) that has a similar modulus as dentin (Modulus 10 GPa). Crowns were fabricated and prepared into the following groups: 24 crowns of translucent zirconia (Lava Esthetic, 3M), 8 bonded with resin cement (Group 1), 8 alumina particle abraded bonded with a resin cement (Group 4) and 8 cemented with resin-modified glass ionomer (Group 7); 24 crowns out of traditional zirconia (Lava Plus, 3M) 8 bonded with resin cement (Group 2), 8 alumina particle abraded bonded with a resin cement (Group 5) and 8 cemented with resin-modified glass ionomer (Group 8); 24 crowns out of lithium disilicate (e.max CAD, Ivoclar Vivadent), 8 bonded with resin cement (Group 3), 8 etched with 5% hydrofluoric acid and silane application bonded with a resin cement (Group 6) and 8 cemented with resin-modified glass ionomer (Group 9). All the crowns were load cycled for 100,000 cycles at 100 N force in a custom fatigue device. Specimens were loaded against a stainless steel ball that made contact with the stylized crowns on each of the four cusps. All fatiguing was performed in 24 C water. The crowns were then fractured in a universal testing machine (MTS). The load was applied with a stainless steel indenter (7mm radius) with a loading rate of 1 mm/min. A 1.5mm rubber sheet was placed between the indenter and the crown to be distributed the load and simulate a food bolus. Results: Lava Plus bonded with self-adhesive resin cement (Group 2) showed the highest values 5383.5 +/- 713.0, followed by Lava Plus with sandblast treatment and bonded with a self-adhesive resin cement (Group 5) 5272.2 +/- 383.2. The lowest value was shown by Lava Esthetic cemented with a RMGI (Group 7) 3007.4 +/- 320.8c. The crowns milled out of e.max CAD (Group 9) failed the during the load cycle test. Conclusions: The strength of Lava Esthetic and e.max CAD are about 2/3 that of Lava Plus when bonded with a resin cement. All materials are strengthened when bonded with a resin cement. When bonded with a resin cement, Lava Esthetic is not weakened with sandblasting. When cemented with a RMGI cement, Lava Esthetic shows a lower fatigue resistance when sandblasted than when sandblasting is omitted. When cemented with a RMGI cement, Lava Esthetic showed a better fatigue resistance than e.max CAD."]},{"key":"dc:description.note","label":"Dc Description Note","values":["etdadmin_upload_568664"]},{"key":"dc:title","label":"Title","values":["Fracture Strength of Translucent Zirconia Crowns"]}]}],"canonical_facts":{"dc:contributor":["Nathaniel Lawson","Daniel Givan","Perng-Ru Liu","Keith Kinderknecht"],"dc:creator":["Jurado, Carlos Alberto"],"dc:date.created":["2018-01-01T08:00:00Z"],"dc:description.abstract":["ABSTRACT Objectives: To measure and compare crown fracture load of a new translucent zirconia. Methods: 72 Standarized crown preparations were designed with AutoCAD software with a 0.8mm shoulder margin and 1 mm incisal-cervical marginal curvature. A stylized crown with a 1mm thickness and 0.8mm minimum thickness in the central pit was designed in 3shape software. Tooth dies were milled out of a resin composite (Crystal Ultra) that has a similar modulus as dentin (Modulus 10 GPa). Crowns were fabricated and prepared into the following groups: 24 crowns of translucent zirconia (Lava Esthetic, 3M), 8 bonded with resin cement (Group 1), 8 alumina particle abraded bonded with a resin cement (Group 4) and 8 cemented with resin-modified glass ionomer (Group 7); 24 crowns out of traditional zirconia (Lava Plus, 3M) 8 bonded with resin cement (Group 2), 8 alumina particle abraded bonded with a resin cement (Group 5) and 8 cemented with resin-modified glass ionomer (Group 8); 24 crowns out of lithium disilicate (e.max CAD, Ivoclar Vivadent), 8 bonded with resin cement (Group 3), 8 etched with 5% hydrofluoric acid and silane application bonded with a resin cement (Group 6) and 8 cemented with resin-modified glass ionomer (Group 9). All the crowns were load cycled for 100,000 cycles at 100 N force in a custom fatigue device. Specimens were loaded against a stainless steel ball that made contact with the stylized crowns on each of the four cusps. All fatiguing was performed in 24 C water. The crowns were then fractured in a universal testing machine (MTS). The load was applied with a stainless steel indenter (7mm radius) with a loading rate of 1 mm/min. A 1.5mm rubber sheet was placed between the indenter and the crown to be distributed the load and simulate a food bolus. Results: Lava Plus bonded with self-adhesive resin cement (Group 2) showed the highest values 5383.5 +/- 713.0, followed by Lava Plus with sandblast treatment and bonded with a self-adhesive resin cement (Group 5) 5272.2 +/- 383.2. The lowest value was shown by Lava Esthetic cemented with a RMGI (Group 7) 3007.4 +/- 320.8c. The crowns milled out of e.max CAD (Group 9) failed the during the load cycle test. Conclusions: The strength of Lava Esthetic and e.max CAD are about 2/3 that of Lava Plus when bonded with a resin cement. All materials are strengthened when bonded with a resin cement. When bonded with a resin cement, Lava Esthetic is not weakened with sandblasting. When cemented with a RMGI cement, Lava Esthetic shows a lower fatigue resistance when sandblasted than when sandblasting is omitted. When cemented with a RMGI cement, Lava Esthetic showed a better fatigue resistance than e.max CAD."],"dc:description.note":["etdadmin_upload_568664"],"dc:identifier":["https://digitalcommons.library.uab.edu/etd-collection/2089"],"dc:subject":["Dentistry"],"dc:title":["Fracture Strength of Translucent Zirconia Crowns"],"thesis:degree_level":["Thesis"]},"updated_at":"2026-11-19T09:26:30Z"}