{"id":{"repo_id":"ubc","oai_identifier":"oai:circle.library.ubc.ca:2429/59418"},"canonical_url":"https://search.ndltd.org/etd/ubc/oai:circle.library.ubc.ca:2429/59418","repository":{"repo_id":"ubc","name":"University of British Columbia","base_url":"http://circle.library.ubc.ca/oai/request"},"display":{"title":"ZnO-based thermoelectrics : modelling, electrochemical thick film growth, and characterization","abstract":"The thermoelectric performance of electrodeposited, aluminum doped zinc oxide was assessed. In this work, wurtzite ZnO was first modelled using Mueller-Plathe to compare the effectiveness of different nanostructured configurations on reducing thermal conductivity. A new analysis technique, Local Vibrational Density of States Equilibrium Molecular Dynamics (LVDOS-EMD), was created to study localized lattice vibrations around nanostructural features of silicon and ZnO, and was used to predict thermal properties in materials of similar composition 17× faster than conventional thermal modelling methods. A 30% void density was determined to yield the best reduction in thermal conductivity by volume of voids in bulk Al:ZnO with a computed thermal conductivity of 0.77 W m-¹ K-¹ at room temperature, 3× below the threshold achieved through established experimental means with high electrical conductivity Al:ZnO. Thick film, electrodeposited Al:ZnO was grown using a nitrate system. Experiments on solution pH using various counter electrodes demonstrated that inert electrodes caused acidification of the growth solution, limiting film thickness. Chloride contamination from commonly used Ag/AgCl reference electrodes was also determined to affect thick film opacity, morphology, crystallinity, and electrical properties. Aluminum integration and activation was explored by adding Al(NO₃)₃ to the growth solution during film synthesis, yielding aluminum integration molar ratios of up to 1.72% (Al.₀₃₄Zn.₉₆₆₀). Partially doped films in excess of 95 µm thick, 4× the thickness reported elsewhere, were electrochemically grown and characterized. Sub-micron voids were integrated into the films using sacrificial material and annealing. A new electrochemical chromium etching methodology was developed and successfully used to free 20 films from their growth substrates for thermoelectric characterization. A new, reusable thermoelectric test apparatus for thin film thermoelectric testing was designed, implemented, calibrated, and successfully deployed to characterize ZnO and Al:ZnO thin films grown 79 – 95 µm in thickness. Extremely low thermal conductivity of 11 mW m-¹ K-¹ at room temperature was demonstrated concurrently with a Seebeck coefficient of -88 µV K-¹. Polycrystallinity and poor dopant activation yielded a low electrical conductivity of 0.75 mS/cm and corresponding low room temperature ZT of 1.3×10-⁵ for the Al:ZnO films.","abstract_html":"The thermoelectric performance of electrodeposited, aluminum doped zinc oxide was assessed. In this work, wurtzite ZnO was first modelled using Mueller-Plathe to compare the effectiveness of different nanostructured configurations on reducing thermal conductivity. A new analysis technique, Local Vibrational Density of States Equilibrium Molecular Dynamics (LVDOS-EMD), was created to study localized lattice vibrations around nanostructural features of silicon and ZnO, and was used to predict thermal properties in materials of similar composition 17× faster than conventional thermal modelling methods. A 30% void density was determined to yield the best reduction in thermal conductivity by volume of voids in bulk Al:ZnO with a computed thermal conductivity of 0.77 W m-¹ K-¹ at room temperature, 3× below the threshold achieved through established experimental means with high electrical conductivity Al:ZnO. Thick film, electrodeposited Al:ZnO was grown using a nitrate system. Experiments on solution pH using various counter electrodes demonstrated that inert electrodes caused acidification of the growth solution, limiting film thickness. Chloride contamination from commonly used Ag/AgCl reference electrodes was also determined to affect thick film opacity, morphology, crystallinity, and electrical properties. Aluminum integration and activation was explored by adding Al(NO₃)₃ to the growth solution during film synthesis, yielding aluminum integration molar ratios of up to 1.72% (Al.₀₃₄Zn.₉₆₆₀). Partially doped films in excess of 95 µm thick, 4× the thickness reported elsewhere, were electrochemically grown and characterized. Sub-micron voids were integrated into the films using sacrificial material and annealing. A new electrochemical chromium etching methodology was developed and successfully used to free 20 films from their growth substrates for thermoelectric characterization. A new, reusable thermoelectric test apparatus for thin film thermoelectric testing was designed, implemented, calibrated, and successfully deployed to characterize ZnO and Al:ZnO thin films grown 79 – 95 µm in thickness. Extremely low thermal conductivity of 11 mW m-¹ K-¹ at room temperature was demonstrated concurrently with a Seebeck coefficient of -88 µV K-¹. Polycrystallinity and poor dopant activation yielded a low electrical conductivity of 0.75 mS/cm and corresponding low room temperature ZT of 1.3×10-⁵ for the Al:ZnO films.","abstract_has_math":false,"creators":["Sielmann, Christoph"],"institution":"University of British Columbia","degree_name":"Doctor of Philosophy - PhD","degree_level":"doctoral","degree_discipline":"Electrical and Computer Engineering","degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2016,"date_issued":"2016","date_published":"2016","updated_at":"2026-11-19T15:00:44Z","subjects":[],"languages":["eng"],"rights":["Attribution-NonCommercial-NoDerivatives 4.0 International"],"rights_urls":["http://creativecommons.org/licenses/by-nc-nd/4.0/"],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://hdl.handle.net/2429/59418","outbound_label":"Handle","outbound_source":"dc:identifier","record_url":"http://hdl.handle.net/2429/59418","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier","download_url":"http://circle.library.ubc.ca/bitstream/2429/59418/4/ubc_2016_november_sielmann_christoph.pdf","download_label":"Download PDF","download_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"http://circle.library.ubc.ca/oai/request?verb=GetRecord&metadataPrefix=etdms&identifier=oai%3Acircle.library.ubc.ca%3A2429%2F59418","prefix":"etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:creator","label":"Author","values":["Sielmann, Christoph"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2016"]},{"key":"dc:publisher","label":"Institution","values":["University of British Columbia"]},{"key":"dc:type","label":"Dc Type","values":["Text"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Electrical and Computer Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["doctoral"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Doctor of Philosophy - PhD"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["University of British Columbia"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["eng"]},{"key":"dc:rights","label":"Dc Rights","values":["http://creativecommons.org/licenses/by-nc-nd/4.0/","Attribution-NonCommercial-NoDerivatives 4.0 International"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://hdl.handle.net/2429/59418","http://circle.library.ubc.ca/bitstream/2429/59418/4/ubc_2016_november_sielmann_christoph.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["The thermoelectric performance of electrodeposited, aluminum doped zinc oxide was assessed. In this work, wurtzite ZnO was first modelled using Mueller-Plathe to compare the effectiveness of different nanostructured configurations on reducing thermal conductivity. A new analysis technique, Local Vibrational Density of States Equilibrium Molecular Dynamics (LVDOS-EMD), was created to study localized lattice vibrations around nanostructural features of silicon and ZnO, and was used to predict thermal properties in materials of similar composition 17× faster than conventional thermal modelling methods. A 30% void density was determined to yield the best reduction in thermal conductivity by volume of voids in bulk Al:ZnO with a computed thermal conductivity of 0.77 W m-¹ K-¹ at room temperature, 3× below the threshold achieved through established experimental means with high electrical conductivity Al:ZnO. Thick film, electrodeposited Al:ZnO was grown using a nitrate system. Experiments on solution pH using various counter electrodes demonstrated that inert electrodes caused acidification of the growth solution, limiting film thickness. Chloride contamination from commonly used Ag/AgCl reference electrodes was also determined to affect thick film opacity, morphology, crystallinity, and electrical properties. Aluminum integration and activation was explored by adding Al(NO₃)₃ to the growth solution during film synthesis, yielding aluminum integration molar ratios of up to 1.72% (Al.₀₃₄Zn.₉₆₆₀). Partially doped films in excess of 95 µm thick, 4× the thickness reported elsewhere, were electrochemically grown and characterized. Sub-micron voids were integrated into the films using sacrificial material and annealing. A new electrochemical chromium etching methodology was developed and successfully used to free 20 films from their growth substrates for thermoelectric characterization. A new, reusable thermoelectric test apparatus for thin film thermoelectric testing was designed, implemented, calibrated, and successfully deployed to characterize ZnO and Al:ZnO thin films grown 79 – 95 µm in thickness. Extremely low thermal conductivity of 11 mW m-¹ K-¹ at room temperature was demonstrated concurrently with a Seebeck coefficient of -88 µV K-¹. Polycrystallinity and poor dopant activation yielded a low electrical conductivity of 0.75 mS/cm and corresponding low room temperature ZT of 1.3×10-⁵ for the Al:ZnO films."]},{"key":"dc:format","label":"Dc Format","values":["20228410","application/pdf"]},{"key":"dc:title","label":"Title","values":["ZnO-based thermoelectrics : modelling, electrochemical thick film growth, and characterization"]}]}],"canonical_facts":{"dc:creator":["Sielmann, Christoph"],"dc:date":["2016"],"dc:description":["The thermoelectric performance of electrodeposited, aluminum doped zinc oxide was assessed. In this work, wurtzite ZnO was first modelled using Mueller-Plathe to compare the effectiveness of different nanostructured configurations on reducing thermal conductivity. A new analysis technique, Local Vibrational Density of States Equilibrium Molecular Dynamics (LVDOS-EMD), was created to study localized lattice vibrations around nanostructural features of silicon and ZnO, and was used to predict thermal properties in materials of similar composition 17× faster than conventional thermal modelling methods. A 30% void density was determined to yield the best reduction in thermal conductivity by volume of voids in bulk Al:ZnO with a computed thermal conductivity of 0.77 W m-¹ K-¹ at room temperature, 3× below the threshold achieved through established experimental means with high electrical conductivity Al:ZnO. Thick film, electrodeposited Al:ZnO was grown using a nitrate system. Experiments on solution pH using various counter electrodes demonstrated that inert electrodes caused acidification of the growth solution, limiting film thickness. Chloride contamination from commonly used Ag/AgCl reference electrodes was also determined to affect thick film opacity, morphology, crystallinity, and electrical properties. Aluminum integration and activation was explored by adding Al(NO₃)₃ to the growth solution during film synthesis, yielding aluminum integration molar ratios of up to 1.72% (Al.₀₃₄Zn.₉₆₆₀). Partially doped films in excess of 95 µm thick, 4× the thickness reported elsewhere, were electrochemically grown and characterized. Sub-micron voids were integrated into the films using sacrificial material and annealing. A new electrochemical chromium etching methodology was developed and successfully used to free 20 films from their growth substrates for thermoelectric characterization. A new, reusable thermoelectric test apparatus for thin film thermoelectric testing was designed, implemented, calibrated, and successfully deployed to characterize ZnO and Al:ZnO thin films grown 79 – 95 µm in thickness. Extremely low thermal conductivity of 11 mW m-¹ K-¹ at room temperature was demonstrated concurrently with a Seebeck coefficient of -88 µV K-¹. Polycrystallinity and poor dopant activation yielded a low electrical conductivity of 0.75 mS/cm and corresponding low room temperature ZT of 1.3×10-⁵ for the Al:ZnO films."],"dc:format":["20228410","application/pdf"],"dc:identifier":["http://hdl.handle.net/2429/59418","http://circle.library.ubc.ca/bitstream/2429/59418/4/ubc_2016_november_sielmann_christoph.pdf"],"dc:language":["eng"],"dc:publisher":["University of British Columbia"],"dc:rights":["http://creativecommons.org/licenses/by-nc-nd/4.0/","Attribution-NonCommercial-NoDerivatives 4.0 International"],"dc:title":["ZnO-based thermoelectrics : modelling, electrochemical thick film growth, and characterization"],"dc:type":["Text"],"thesis:degree_discipline":["Electrical and Computer Engineering"],"thesis:degree_level":["doctoral"],"thesis:degree_name":["Doctor of Philosophy - PhD"],"thesis:institution_name":["University of British Columbia"]},"updated_at":"2026-11-19T15:00:44Z"}