{"id":{"repo_id":"ubc","oai_identifier":"oai:circle.library.ubc.ca:2429/72208"},"canonical_url":"https://search.ndltd.org/etd/ubc/oai:circle.library.ubc.ca:2429/72208","repository":{"repo_id":"ubc","name":"University of British Columbia","base_url":"http://circle.library.ubc.ca/oai/request"},"display":{"title":"A study of selenate removal from water by adsorption on an aged, carbonated Friedel’s salt material with mass loss considerations","abstract":"In this work, selenate removal from water was studied using a material from the layered double hydroxide family. This material is a mixture of two hydrocalumite phases, chloro-hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl₂·4H₂O] and chloro-carboaluminate hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl(CO₃)₀.₅·10.8H₂O]. This material is called aged-FS in this thesis. Aged-FS was obtained by the co-precipitation method followed by an aging process. The aging condition was initial pH 12.0, liquid/solid ratio 20, 65 °C, for 7 days. During aging, a phase transformation from chloro-hydrocalumite in the hexagonal crystal system to chloro-carboaluminate hydrocalumite in the monoclinic crystal system was observed. The aluminum hydroxide impurity was removed and katoite (Ca3Al2(OH)12) was formed. The formation of well-shaped hexagon crystallites and agglomeration of particles were observed by morphology and particle size studies, respectively. The carbonate content increased during aging from 1.15 to 3.00 wt.%. By aging, ~50% reduction in FS dissolution was recorded. By some modifications in nitrogen purging of the synthesis process, the carbonate content was reduced from 1.15 to 1.01 wt.%. For selenate removal studies, the effect of initial pH, liquid/solid ratio, time, temperature, agitation, selenate concentration, sulfate and carbonate interference, and container type were studied. The highest loading percentage of selenate and the lowest dissolution of aged-FS was achieved at initial pH 12.0, liquid/solid ratio 200, 30 °C, 24 h, and 150 RPM. A selenate loading isotherm was fitted to the Langmuir model with maximum loading of 71.1 mg Se/g. The intercalated carbonate in aged-FS did not interfere with selenate removal while significant interference was observed from carbonate in solution. The sulfate anion did not interfere with selenate adsorption. The Al dissolution from aged-FS in an adsorption test was suppressed using calcium hydroxide solution. The Al concentration reached to 0.07 ppm; a value lower than the maximum instantaneous value set by a BC guideline. Calcination of aged-FS improved the selenate loading. The lowest level of selenium in solution achieved using the calcined aged-FS (1.84 ppb) met the 2016 US EPA maximum discharge limit of lotic water for Se (<3.1 ppb). Overall, calcined aged-FS is a promising exchanger for selenate removal from calcium sulfate- saturated industrial effluents.","abstract_html":"In this work, selenate removal from water was studied using a material from the layered double hydroxide family. This material is a mixture of two hydrocalumite phases, chloro-hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl₂·4H₂O] and chloro-carboaluminate hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl(CO₃)₀.₅·10.8H₂O]. This material is called aged-FS in this thesis. Aged-FS was obtained by the co-precipitation method followed by an aging process. The aging condition was initial pH 12.0, liquid/solid ratio 20, 65 °C, for 7 days. During aging, a phase transformation from chloro-hydrocalumite in the hexagonal crystal system to chloro-carboaluminate hydrocalumite in the monoclinic crystal system was observed. The aluminum hydroxide impurity was removed and katoite (Ca3Al2(OH)12) was formed. The formation of well-shaped hexagon crystallites and agglomeration of particles were observed by morphology and particle size studies, respectively. The carbonate content increased during aging from 1.15 to 3.00 wt.%. By aging, ~50% reduction in FS dissolution was recorded. By some modifications in nitrogen purging of the synthesis process, the carbonate content was reduced from 1.15 to 1.01 wt.%. For selenate removal studies, the effect of initial pH, liquid/solid ratio, time, temperature, agitation, selenate concentration, sulfate and carbonate interference, and container type were studied. The highest loading percentage of selenate and the lowest dissolution of aged-FS was achieved at initial pH 12.0, liquid/solid ratio 200, 30 °C, 24 h, and 150 RPM. A selenate loading isotherm was fitted to the Langmuir model with maximum loading of 71.1 mg Se/g. The intercalated carbonate in aged-FS did not interfere with selenate removal while significant interference was observed from carbonate in solution. The sulfate anion did not interfere with selenate adsorption. The Al dissolution from aged-FS in an adsorption test was suppressed using calcium hydroxide solution. The Al concentration reached to 0.07 ppm; a value lower than the maximum instantaneous value set by a BC guideline. Calcination of aged-FS improved the selenate loading. The lowest level of selenium in solution achieved using the calcined aged-FS (1.84 ppb) met the 2016 US EPA maximum discharge limit of lotic water for Se (&lt;3.1 ppb). Overall, calcined aged-FS is a promising exchanger for selenate removal from calcium sulfate- saturated industrial effluents.","abstract_has_math":false,"creators":["Rasouli, Maryam"],"institution":"University of British Columbia","degree_name":"Doctor of Philosophy - PhD","degree_level":"doctoral","degree_discipline":"Materials Engineering","degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2019,"date_issued":"2019","date_published":"2019","updated_at":"2026-11-19T15:11:19Z","subjects":[],"languages":["eng"],"rights":["Attribution-NonCommercial-NoDerivatives 4.0 International"],"rights_urls":["http://creativecommons.org/licenses/by-nc-nd/4.0/"],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://hdl.handle.net/2429/72208","outbound_label":"Handle","outbound_source":"dc:identifier","record_url":"http://hdl.handle.net/2429/72208","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier","download_url":"http://circle.library.ubc.ca/bitstream/2429/72208/1/ubc_2020_may_rasouli_maryam.pdf","download_label":"Download PDF","download_source":"dc:identifier","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"http://circle.library.ubc.ca/oai/request?verb=GetRecord&metadataPrefix=etdms&identifier=oai%3Acircle.library.ubc.ca%3A2429%2F72208","prefix":"etdms"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:creator","label":"Author","values":["Rasouli, Maryam"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2019"]},{"key":"dc:publisher","label":"Institution","values":["University of British Columbia"]},{"key":"dc:type","label":"Dc Type","values":["Text"]},{"key":"thesis:degree_discipline","label":"Discipline","values":["Materials Engineering"]},{"key":"thesis:degree_level","label":"Degree Level","values":["doctoral"]},{"key":"thesis:degree_name","label":"Degree Name","values":["Doctor of Philosophy - PhD"]},{"key":"thesis:institution_name","label":"Thesis Institution Name","values":["University of British Columbia"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["eng"]},{"key":"dc:rights","label":"Dc Rights","values":["http://creativecommons.org/licenses/by-nc-nd/4.0/","Attribution-NonCommercial-NoDerivatives 4.0 International"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["http://hdl.handle.net/2429/72208","http://circle.library.ubc.ca/bitstream/2429/72208/1/ubc_2020_may_rasouli_maryam.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["In this work, selenate removal from water was studied using a material from the layered double hydroxide family. This material is a mixture of two hydrocalumite phases, chloro-hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl₂·4H₂O] and chloro-carboaluminate hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl(CO₃)₀.₅·10.8H₂O]. This material is called aged-FS in this thesis. Aged-FS was obtained by the co-precipitation method followed by an aging process. The aging condition was initial pH 12.0, liquid/solid ratio 20, 65 °C, for 7 days. During aging, a phase transformation from chloro-hydrocalumite in the hexagonal crystal system to chloro-carboaluminate hydrocalumite in the monoclinic crystal system was observed. The aluminum hydroxide impurity was removed and katoite (Ca3Al2(OH)12) was formed. The formation of well-shaped hexagon crystallites and agglomeration of particles were observed by morphology and particle size studies, respectively. The carbonate content increased during aging from 1.15 to 3.00 wt.%. By aging, ~50% reduction in FS dissolution was recorded. By some modifications in nitrogen purging of the synthesis process, the carbonate content was reduced from 1.15 to 1.01 wt.%. For selenate removal studies, the effect of initial pH, liquid/solid ratio, time, temperature, agitation, selenate concentration, sulfate and carbonate interference, and container type were studied. The highest loading percentage of selenate and the lowest dissolution of aged-FS was achieved at initial pH 12.0, liquid/solid ratio 200, 30 °C, 24 h, and 150 RPM. A selenate loading isotherm was fitted to the Langmuir model with maximum loading of 71.1 mg Se/g. The intercalated carbonate in aged-FS did not interfere with selenate removal while significant interference was observed from carbonate in solution. The sulfate anion did not interfere with selenate adsorption. The Al dissolution from aged-FS in an adsorption test was suppressed using calcium hydroxide solution. The Al concentration reached to 0.07 ppm; a value lower than the maximum instantaneous value set by a BC guideline. Calcination of aged-FS improved the selenate loading. The lowest level of selenium in solution achieved using the calcined aged-FS (1.84 ppb) met the 2016 US EPA maximum discharge limit of lotic water for Se (<3.1 ppb). Overall, calcined aged-FS is a promising exchanger for selenate removal from calcium sulfate- saturated industrial effluents."]},{"key":"dc:format","label":"Dc Format","values":["5064050","application/pdf"]},{"key":"dc:title","label":"Title","values":["A study of selenate removal from water by adsorption on an aged, carbonated Friedel’s salt material with mass loss considerations"]}]}],"canonical_facts":{"dc:creator":["Rasouli, Maryam"],"dc:date":["2019"],"dc:description":["In this work, selenate removal from water was studied using a material from the layered double hydroxide family. This material is a mixture of two hydrocalumite phases, chloro-hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl₂·4H₂O] and chloro-carboaluminate hydrocalumite [Ca₄Al₂(OH)₁₂]·[Cl(CO₃)₀.₅·10.8H₂O]. This material is called aged-FS in this thesis. Aged-FS was obtained by the co-precipitation method followed by an aging process. The aging condition was initial pH 12.0, liquid/solid ratio 20, 65 °C, for 7 days. During aging, a phase transformation from chloro-hydrocalumite in the hexagonal crystal system to chloro-carboaluminate hydrocalumite in the monoclinic crystal system was observed. The aluminum hydroxide impurity was removed and katoite (Ca3Al2(OH)12) was formed. The formation of well-shaped hexagon crystallites and agglomeration of particles were observed by morphology and particle size studies, respectively. The carbonate content increased during aging from 1.15 to 3.00 wt.%. By aging, ~50% reduction in FS dissolution was recorded. By some modifications in nitrogen purging of the synthesis process, the carbonate content was reduced from 1.15 to 1.01 wt.%. For selenate removal studies, the effect of initial pH, liquid/solid ratio, time, temperature, agitation, selenate concentration, sulfate and carbonate interference, and container type were studied. The highest loading percentage of selenate and the lowest dissolution of aged-FS was achieved at initial pH 12.0, liquid/solid ratio 200, 30 °C, 24 h, and 150 RPM. A selenate loading isotherm was fitted to the Langmuir model with maximum loading of 71.1 mg Se/g. The intercalated carbonate in aged-FS did not interfere with selenate removal while significant interference was observed from carbonate in solution. The sulfate anion did not interfere with selenate adsorption. The Al dissolution from aged-FS in an adsorption test was suppressed using calcium hydroxide solution. The Al concentration reached to 0.07 ppm; a value lower than the maximum instantaneous value set by a BC guideline. Calcination of aged-FS improved the selenate loading. The lowest level of selenium in solution achieved using the calcined aged-FS (1.84 ppb) met the 2016 US EPA maximum discharge limit of lotic water for Se (<3.1 ppb). Overall, calcined aged-FS is a promising exchanger for selenate removal from calcium sulfate- saturated industrial effluents."],"dc:format":["5064050","application/pdf"],"dc:identifier":["http://hdl.handle.net/2429/72208","http://circle.library.ubc.ca/bitstream/2429/72208/1/ubc_2020_may_rasouli_maryam.pdf"],"dc:language":["eng"],"dc:publisher":["University of British Columbia"],"dc:rights":["http://creativecommons.org/licenses/by-nc-nd/4.0/","Attribution-NonCommercial-NoDerivatives 4.0 International"],"dc:title":["A study of selenate removal from water by adsorption on an aged, carbonated Friedel’s salt material with mass loss considerations"],"dc:type":["Text"],"thesis:degree_discipline":["Materials Engineering"],"thesis:degree_level":["doctoral"],"thesis:degree_name":["Doctor of Philosophy - PhD"],"thesis:institution_name":["University of British Columbia"]},"updated_at":"2026-11-19T15:11:19Z"}