{"id":{"repo_id":"ucl","oai_identifier":"oai:eprints.ucl.ac.uk.OAI2:10231210"},"canonical_url":"https://search.ndltd.org/etd/ucl/oai:eprints.ucl.ac.uk.OAI2:10231210","repository":{"repo_id":"ucl","name":"University College London","base_url":"https://discovery.ucl.ac.uk/cgi/oai2"},"display":{"title":"Conditions for the safe storage of early glass","abstract":"It is generally agreed that glass deteriorates through interaction with water and is subsequently left with a hydrated, low-density, silica-rich surface layer. Eventually, excessively humid conditions may trigger ‘crizzling’- a damaging phenomenon defined by microcrack formation and flaking. This transformed surface eventually delaminates, and the entire object gradually disintegrates in storage unless the ambient RH is sufficiently low. Unfortunately, crizzling can also be caused by deteriorated glass drying. This study focuses on establishing a balanced RH figure where the humidity-induced changes to pristine glass are slowed while the risk of irreversible altered glass desiccation is minimised. This is done by means of direct observation of experimentally aged glass replicas subjected to various environmental changes. An initial series of studies evaluated artificial ageing media, including water, acidic, and mildly alkaline solutions. The latter was found to be the most effective for rapidly reproducing altered layers consistent with archaeological specimens. These aged samples were subjected to a multi-faceted analytical approach. Initially, Dynamic Vapour Sorption (DVS) analysis was performed on both the model and authentic archaeological glass coupons. The principal experiment then entailed the long-term (c. one year) storage of aged coupons at 30°C across a 20% to 60% RH range. The resulting crizzling progression was quantified by counting flakes in ‘before’ and ‘after’ microphotographs. The results achieved by this research demonstrate that there is a statistically significant negative correlation between RH and new crack formation, with damage increasing as RH decreases. The DVS and long-term storage data aligned, identifying a sharp increase in mass loss and crizzling in samples stored at or below 35% RH. This study therefore provides empirical evidence for the lowest acceptable RH level for the storage and display of altered glass. The project provides updated guidelines for glass storage to be used by ancient glass custodians across heritage collections and institutions.","abstract_html":"It is generally agreed that glass deteriorates through interaction with water and is subsequently left with a hydrated, low-density, silica-rich surface layer. Eventually, excessively humid conditions may trigger ‘crizzling’- a damaging phenomenon defined by microcrack formation and flaking. This transformed surface eventually delaminates, and the entire object gradually disintegrates in storage unless the ambient RH is sufficiently low. Unfortunately, crizzling can also be caused by deteriorated glass drying. This study focuses on establishing a balanced RH figure where the humidity-induced changes to pristine glass are slowed while the risk of irreversible altered glass desiccation is minimised. This is done by means of direct observation of experimentally aged glass replicas subjected to various environmental changes. An initial series of studies evaluated artificial ageing media, including water, acidic, and mildly alkaline solutions. The latter was found to be the most effective for rapidly reproducing altered layers consistent with archaeological specimens. These aged samples were subjected to a multi-faceted analytical approach. Initially, Dynamic Vapour Sorption (DVS) analysis was performed on both the model and authentic archaeological glass coupons. The principal experiment then entailed the long-term (c. one year) storage of aged coupons at 30°C across a 20% to 60% RH range. The resulting crizzling progression was quantified by counting flakes in ‘before’ and ‘after’ microphotographs. The results achieved by this research demonstrate that there is a statistically significant negative correlation between RH and new crack formation, with damage increasing as RH decreases. The DVS and long-term storage data aligned, identifying a sharp increase in mass loss and crizzling in samples stored at or below 35% RH. This study therefore provides empirical evidence for the lowest acceptable RH level for the storage and display of altered glass. The project provides updated guidelines for glass storage to be used by ancient glass custodians across heritage collections and institutions.","abstract_has_math":false,"creators":["Melinis, Antanas"],"institution":"UCL (University College London)","degree_name":null,"degree_level":"Doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2026,"date_issued":"2026-09","date_published":"2026-09","updated_at":"2026-11-26T07:44:34Z","subjects":[],"languages":["en","eng"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"https://discovery.ucl.ac.uk/id/eprint/10231210/","outbound_label":"Repository record","outbound_source":"dc:identifier.uri","record_url":"https://discovery.ucl.ac.uk/id/eprint/10231210/","record_label":"Repository record","record_kind":"record","record_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aucl%3Aoai%3Aeprints.ucl.ac.uk.OAI2%3A10231210","prefix":"oai_dc"},"source_record":{"url":"https://discovery.ucl.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aeprints.ucl.ac.uk.OAI2%3A10231210","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:creator","label":"Author","values":["Melinis, Antanas"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2026-09-28"]},{"key":"dc:date.issued","label":"Date","values":["2026-09"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Institute of Archaeology"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["UCL (University College London)"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["Doctoral"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language","label":"Dc Language","values":["en","eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://discovery.ucl.ac.uk/id/eprint/10231210/"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["It is generally agreed that glass deteriorates through interaction with water and is subsequently left with a hydrated, low-density, silica-rich surface layer. Eventually, excessively humid conditions may trigger ‘crizzling’- a damaging phenomenon defined by microcrack formation and flaking. This transformed surface eventually delaminates, and the entire object gradually disintegrates in storage unless the ambient RH is sufficiently low. Unfortunately, crizzling can also be caused by deteriorated glass drying. This study focuses on establishing a balanced RH figure where the humidity-induced changes to pristine glass are slowed while the risk of irreversible altered glass desiccation is minimised. This is done by means of direct observation of experimentally aged glass replicas subjected to various environmental changes. An initial series of studies evaluated artificial ageing media, including water, acidic, and mildly alkaline solutions. The latter was found to be the most effective for rapidly reproducing altered layers consistent with archaeological specimens. These aged samples were subjected to a multi-faceted analytical approach. Initially, Dynamic Vapour Sorption (DVS) analysis was performed on both the model and authentic archaeological glass coupons. The principal experiment then entailed the long-term (c. one year) storage of aged coupons at 30°C across a 20% to 60% RH range. The resulting crizzling progression was quantified by counting flakes in ‘before’ and ‘after’ microphotographs. The results achieved by this research demonstrate that there is a statistically significant negative correlation between RH and new crack formation, with damage increasing as RH decreases. The DVS and long-term storage data aligned, identifying a sharp increase in mass loss and crizzling in samples stored at or below 35% RH. This study therefore provides empirical evidence for the lowest acceptable RH level for the storage and display of altered glass. The project provides updated guidelines for glass storage to be used by ancient glass custodians across heritage collections and institutions."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Conditions for the safe storage of early glass"]}]}],"canonical_facts":{"dc:creator":["Melinis, Antanas"],"dc:date":["2026-09-28"],"dc:date.issued":["2026-09"],"dc:description.abstract":["It is generally agreed that glass deteriorates through interaction with water and is subsequently left with a hydrated, low-density, silica-rich surface layer. Eventually, excessively humid conditions may trigger ‘crizzling’- a damaging phenomenon defined by microcrack formation and flaking. This transformed surface eventually delaminates, and the entire object gradually disintegrates in storage unless the ambient RH is sufficiently low. Unfortunately, crizzling can also be caused by deteriorated glass drying. This study focuses on establishing a balanced RH figure where the humidity-induced changes to pristine glass are slowed while the risk of irreversible altered glass desiccation is minimised. This is done by means of direct observation of experimentally aged glass replicas subjected to various environmental changes. An initial series of studies evaluated artificial ageing media, including water, acidic, and mildly alkaline solutions. The latter was found to be the most effective for rapidly reproducing altered layers consistent with archaeological specimens. These aged samples were subjected to a multi-faceted analytical approach. Initially, Dynamic Vapour Sorption (DVS) analysis was performed on both the model and authentic archaeological glass coupons. The principal experiment then entailed the long-term (c. one year) storage of aged coupons at 30°C across a 20% to 60% RH range. The resulting crizzling progression was quantified by counting flakes in ‘before’ and ‘after’ microphotographs. The results achieved by this research demonstrate that there is a statistically significant negative correlation between RH and new crack formation, with damage increasing as RH decreases. The DVS and long-term storage data aligned, identifying a sharp increase in mass loss and crizzling in samples stored at or below 35% RH. This study therefore provides empirical evidence for the lowest acceptable RH level for the storage and display of altered glass. The project provides updated guidelines for glass storage to be used by ancient glass custodians across heritage collections and institutions."],"dc:format":["text"],"dc:identifier.uri":["https://discovery.ucl.ac.uk/id/eprint/10231210/"],"dc:language":["en","eng"],"dc:publisher.department":["Institute of Archaeology"],"dc:publisher.institution":["UCL (University College London)"],"dcterms:accessrights":["public"],"dc:title":["Conditions for the safe storage of early glass"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["Doctoral"]},"updated_at":"2026-11-26T07:44:34Z"}