{"id":{"repo_id":"ukzn","oai_identifier":"oai:researchspace.ukzn.ac.za:10413/11801"},"canonical_url":"https://search.ndltd.org/etd/ukzn/oai:researchspace.ukzn.ac.za:10413/11801","repository":{"repo_id":"ukzn","name":"University of Kwazulu-Natal","base_url":"https://researchspace.ukzn.ac.za/server/oai/request"},"display":{"title":"Structure and bi-magnetism of nanocomposites and nanoalloys synthesized by reduction of (Co, Ni) Fe2O4 nano-ferrites.","abstract":"Structural and magnetic properties of CoFe2O4, NiFe2O4 nano-ferrites, CoFe2O4 /CoFe2, NiFe2O4/NiFe bi-magnetic nanocomposites and CoFe2, NiFe alloys were studied. The nano-ferrites were synthesised using the glycol-thermal method at 200 C for 6 hours. The nanocomposites and alloys were produced by the reduction of the ferrites using di erent amounts of activated charcoal. The reduction reaction was performed at 900 C for 3 hours in high purity owing argon atmosphere. Complete reduction yields the alloy phases while partial reduction produces the nanocomposites. The samples were studied using X-ray di raction (XRD), high resolution transmission electron microscopy (HRTEM), high resolution scanning electron microscopy (HRSEM), 57Fe M ossbauer spectroscopy, LakeShore vibrating sample magnetometer and a mini cryogen free system. XRD measurements of the nano-ferrites showed a single phase spinel structure with average crystallite sizes of about 10 nm. the CoFe2 alloy was obtained at an activated charcoal to ferrite molar ratio nC = 6 while the NiFe alloy was obtained at nC = 5. XRD results of the reduced samples of NiFe2O4 showed the coexistence of bcc -Fe and fcc -Fe lattice structures for NiFe alloy. The HRTEM and HRSEM measurements of all the reduced samples showed clear di erences between the morphology of the parent nano-ferrites and the reduced samples. 57Fe M ossbauer spectra measurements of the reduced samples showed the transformation of the spinel structure to the alloy phase. The presence of mixed phases in the nanocomposites was revealed. A small amount of mixed phase in CoFe2 and NiFe alloys which was not detected by XRD was revealed by M ossbauer measurement for nC = 6 and nC = 5 respectively. The M ossbauer ts showed that Fe3+ was reduced to Fe2+ with lower magnetic hyper ne elds observed in the reduced samples. High eld (50 kOe) magnetization measurements at room temperature for CoFe2O4/CoFe2 nanocomposite show signi cant enhancement of saturation magnetization from 63 emu/g of the parent nano-ferrite to 221 emu/g at nC = 5. In the NiFe2O4/NiFe nanocomposite the in magnetization increased from 57 emu/g to 141 emu/g at nC = 6. Low temperature measurements performed on the nanocomposites exhibited higher magnetizations. The coercivity of the fully reduced samples of the nano-ferrites were observed to be less dependent on temperature.","abstract_html":"Structural and magnetic properties of CoFe2O4, NiFe2O4 nano-ferrites, CoFe2O4 /CoFe2, NiFe2O4/NiFe bi-magnetic nanocomposites and CoFe2, NiFe alloys were studied. The nano-ferrites were synthesised using the glycol-thermal method at 200 C for 6 hours. The nanocomposites and alloys were produced by the reduction of the ferrites using di erent amounts of activated charcoal. The reduction reaction was performed at 900 C for 3 hours in high purity owing argon atmosphere. Complete reduction yields the alloy phases while partial reduction produces the nanocomposites. The samples were studied using X-ray di raction (XRD), high resolution transmission electron microscopy (HRTEM), high resolution scanning electron microscopy (HRSEM), 57Fe M ossbauer spectroscopy, LakeShore vibrating sample magnetometer and a mini cryogen free system. XRD measurements of the nano-ferrites showed a single phase spinel structure with average crystallite sizes of about 10 nm. the CoFe2 alloy was obtained at an activated charcoal to ferrite molar ratio nC = 6 while the NiFe alloy was obtained at nC = 5. XRD results of the reduced samples of NiFe2O4 showed the coexistence of bcc -Fe and fcc -Fe lattice structures for NiFe alloy. The HRTEM and HRSEM measurements of all the reduced samples showed clear di erences between the morphology of the parent nano-ferrites and the reduced samples. 57Fe M ossbauer spectra measurements of the reduced samples showed the transformation of the spinel structure to the alloy phase. The presence of mixed phases in the nanocomposites was revealed. A small amount of mixed phase in CoFe2 and NiFe alloys which was not detected by XRD was revealed by M ossbauer measurement for nC = 6 and nC = 5 respectively. The M ossbauer ts showed that Fe3+ was reduced to Fe2+ with lower magnetic hyper ne elds observed in the reduced samples. High eld (50 kOe) magnetization measurements at room temperature for CoFe2O4/CoFe2 nanocomposite show signi cant enhancement of saturation magnetization from 63 emu/g of the parent nano-ferrite to 221 emu/g at nC = 5. In the NiFe2O4/NiFe nanocomposite the in magnetization increased from 57 emu/g to 141 emu/g at nC = 6. Low temperature measurements performed on the nanocomposites exhibited higher magnetizations. The coercivity of the fully reduced samples of the nano-ferrites were observed to be less dependent on temperature.","abstract_has_math":false,"creators":["Ezekiel, Itegbeyogene Patrick."],"institution":null,"degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Moyo, Thomas."],"committee_chairs":[],"committee_members":[],"year":2014,"date_issued":"2014","date_published":"2014","updated_at":"2026-11-27T09:16:12Z","subjects":["Nanocomposites (Materials)","Ferrites (Magnetic materials)","Ferrimagnetism.","Ferromagnetism.","Magnetism.","Alloys.","Theses--Physics."],"languages":["en_ZA"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"https://hdl.handle.net/10413/11801","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"https://hdl.handle.net/10413/11801","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"oai_pmh_record":{"url":"https://union.ndltd.org/oai-pmh/?verb=GetRecord&metadataPrefix=oai_dc&identifier=oai%3Aunion.ndltd.org%3Arepo%3Aukzn%3Aoai%3Aresearchspace.ukzn.ac.za%3A10413%2F11801","prefix":"oai_dc"},"source_record":{"url":"https://researchspace.ukzn.ac.za/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Aresearchspace.ukzn.ac.za%3A10413%2F11801","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Moyo, Thomas."]},{"key":"dc:creator","label":"Author","values":["Ezekiel, Itegbeyogene Patrick."]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2015-01-05T07:12:17Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2015-01-05T07:12:17Z"]},{"key":"dc:date.created","label":"Dc Date Created","values":["2014"]},{"key":"dc:date.issued","label":"Date","values":["2014"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["Nanocomposites (Materials)","Ferrites (Magnetic materials)","Ferrimagnetism.","Ferromagnetism.","Magnetism.","Alloys.","Theses--Physics."]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.iso","label":"Language (ISO)","values":["en_ZA"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["http://hdl.handle.net/10413/11801"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description","label":"Description","values":["M. Sc. University of KwaZulu-Natal, Durban 2014."]},{"key":"dc:description.abstract","label":"Abstract","values":["Structural and magnetic properties of CoFe2O4, NiFe2O4 nano-ferrites, CoFe2O4 /CoFe2, NiFe2O4/NiFe bi-magnetic nanocomposites and CoFe2, NiFe alloys were studied. The nano-ferrites were synthesised using the glycol-thermal method at 200 C for 6 hours. The nanocomposites and alloys were produced by the reduction of the ferrites using di erent amounts of activated charcoal. The reduction reaction was performed at 900 C for 3 hours in high purity owing argon atmosphere. Complete reduction yields the alloy phases while partial reduction produces the nanocomposites. The samples were studied using X-ray di raction (XRD), high resolution transmission electron microscopy (HRTEM), high resolution scanning electron microscopy (HRSEM), 57Fe M ossbauer spectroscopy, LakeShore vibrating sample magnetometer and a mini cryogen free system. XRD measurements of the nano-ferrites showed a single phase spinel structure with average crystallite sizes of about 10 nm. the CoFe2 alloy was obtained at an activated charcoal to ferrite molar ratio nC = 6 while the NiFe alloy was obtained at nC = 5. XRD results of the reduced samples of NiFe2O4 showed the coexistence of bcc -Fe and fcc -Fe lattice structures for NiFe alloy. The HRTEM and HRSEM measurements of all the reduced samples showed clear di erences between the morphology of the parent nano-ferrites and the reduced samples. 57Fe M ossbauer spectra measurements of the reduced samples showed the transformation of the spinel structure to the alloy phase. The presence of mixed phases in the nanocomposites was revealed. A small amount of mixed phase in CoFe2 and NiFe alloys which was not detected by XRD was revealed by M ossbauer measurement for nC = 6 and nC = 5 respectively. The M ossbauer ts showed that Fe3+ was reduced to Fe2+ with lower magnetic hyper ne elds observed in the reduced samples. High eld (50 kOe) magnetization measurements at room temperature for CoFe2O4/CoFe2 nanocomposite show signi cant enhancement of saturation magnetization from 63 emu/g of the parent nano-ferrite to 221 emu/g at nC = 5. In the NiFe2O4/NiFe nanocomposite the in magnetization increased from 57 emu/g to 141 emu/g at nC = 6. Low temperature measurements performed on the nanocomposites exhibited higher magnetizations. The coercivity of the fully reduced samples of the nano-ferrites were observed to be less dependent on temperature."]},{"key":"dc:title","label":"Title","values":["Structure and bi-magnetism of nanocomposites and nanoalloys synthesized by reduction of (Co, Ni) Fe2O4 nano-ferrites."]},{"key":"others:access_status","label":"Others Access Status","values":["open.access"]}]}],"canonical_facts":{"dc:contributor.advisor":["Moyo, Thomas."],"dc:creator":["Ezekiel, Itegbeyogene Patrick."],"dc:date.accessioned":["2015-01-05T07:12:17Z"],"dc:date.available":["2015-01-05T07:12:17Z"],"dc:date.created":["2014"],"dc:date.issued":["2014"],"dc:description":["M. Sc. University of KwaZulu-Natal, Durban 2014."],"dc:description.abstract":["Structural and magnetic properties of CoFe2O4, NiFe2O4 nano-ferrites, CoFe2O4 /CoFe2, NiFe2O4/NiFe bi-magnetic nanocomposites and CoFe2, NiFe alloys were studied. The nano-ferrites were synthesised using the glycol-thermal method at 200 C for 6 hours. The nanocomposites and alloys were produced by the reduction of the ferrites using di erent amounts of activated charcoal. The reduction reaction was performed at 900 C for 3 hours in high purity owing argon atmosphere. Complete reduction yields the alloy phases while partial reduction produces the nanocomposites. The samples were studied using X-ray di raction (XRD), high resolution transmission electron microscopy (HRTEM), high resolution scanning electron microscopy (HRSEM), 57Fe M ossbauer spectroscopy, LakeShore vibrating sample magnetometer and a mini cryogen free system. XRD measurements of the nano-ferrites showed a single phase spinel structure with average crystallite sizes of about 10 nm. the CoFe2 alloy was obtained at an activated charcoal to ferrite molar ratio nC = 6 while the NiFe alloy was obtained at nC = 5. XRD results of the reduced samples of NiFe2O4 showed the coexistence of bcc -Fe and fcc -Fe lattice structures for NiFe alloy. The HRTEM and HRSEM measurements of all the reduced samples showed clear di erences between the morphology of the parent nano-ferrites and the reduced samples. 57Fe M ossbauer spectra measurements of the reduced samples showed the transformation of the spinel structure to the alloy phase. The presence of mixed phases in the nanocomposites was revealed. A small amount of mixed phase in CoFe2 and NiFe alloys which was not detected by XRD was revealed by M ossbauer measurement for nC = 6 and nC = 5 respectively. The M ossbauer ts showed that Fe3+ was reduced to Fe2+ with lower magnetic hyper ne elds observed in the reduced samples. High eld (50 kOe) magnetization measurements at room temperature for CoFe2O4/CoFe2 nanocomposite show signi cant enhancement of saturation magnetization from 63 emu/g of the parent nano-ferrite to 221 emu/g at nC = 5. In the NiFe2O4/NiFe nanocomposite the in magnetization increased from 57 emu/g to 141 emu/g at nC = 6. Low temperature measurements performed on the nanocomposites exhibited higher magnetizations. The coercivity of the fully reduced samples of the nano-ferrites were observed to be less dependent on temperature."],"dc:identifier.uri":["http://hdl.handle.net/10413/11801"],"dc:language.iso":["en_ZA"],"dc:subject":["Nanocomposites (Materials)","Ferrites (Magnetic materials)","Ferrimagnetism.","Ferromagnetism.","Magnetism.","Alloys.","Theses--Physics."],"dc:title":["Structure and bi-magnetism of nanocomposites and nanoalloys synthesized by reduction of (Co, Ni) Fe2O4 nano-ferrites."],"dc:type":["Thesis"],"others:access_status":["open.access"]},"updated_at":"2026-11-27T09:16:12Z"}