{"id":{"repo_id":"waterloo","oai_identifier":"oai:uwspace.uwaterloo.ca:10012/7181"},"canonical_url":"https://search.ndltd.org/etd/waterloo/oai:uwspace.uwaterloo.ca:10012/7181","repository":{"repo_id":"waterloo","name":"University of Waterloo","base_url":"https://dspacemainprd01.lib.uwaterloo.ca/server/oai/request"},"display":{"title":"Behaviour of Mesoporous Silica (MCM-41) Supported Catalysts in Degradation Reactions","abstract":"A research project was carried out to investigate several aspects of Mobil’s composition of matter #41 (MCM-41) pertaining to its potential application in water treatment technologies. The goal of the work was to lead to a recommendation of whether further work investigating this particular, potential application is warranted at the present time. A dissolution experiment indicated that Pd/MCM-41 is more stable in contact with deionized water at 25±0.1 degrees Celsius than purely siliceous MCM-41. Stability increases with increasing mass percent loading of Pd in the Pd/MCM-41 material. The increased stability was attributed to a reduction in Pd/MCM-41 surface areas relative to the parent MCM-41 material. The reduction in surface area is likely the result of partial or complete blocking of the MCM-41 mesopores by Pd centres. Ni/MCM-41 was less stable in contact with deionized water than MCM-41 and Pd/MCM-41. Both Ni and Pd impregnated MCM-41 exhibited enhanced stability relative to purely siliceous MCM-41 in 0.01 M NaCl solution. The stability enhancement was more pronounced for Pd/MCM-41. A long term dissolution experiment showed that MCM-41 retained its characteristic hexagonal mesopore structure and high surface area after 1,174 days of contact with deionized water. The ability of Pd/MCM-41 to absorb hydrogen was investigated in a series of experiments in pressure cells at 25±0.1 degrees Celsius and approximately 101.3 kPa. The Pd in Pd/MCM-41 was able to absorb 0.85±0.18 moles of hydrogen per mole of Pd present. This was a higher level of absorption than found in most other, published Pd-hydrogen investigations. It is proposed that enhanced uptake of hydrogen by Pd/MCM-41 may be the result of a higher proportion of surface and subsurface sites in the samples relative to other supported Pd materials. Batch and column trichloroethylene (TCE) degradation experiments indicated that Pd/MCM-41 has substantial longevity while degrading at least 91% of inflow TCE concentrations in hydrogen-saturated deionized water over 5,036 pore volumes. The average inflow TCE concentration was 4.94E-2 ± 4.87E-3 mmol/l with maximum and minimum concentrations of 7.24E-2 mmol/l and 2.63E-2 mmol/l, respectively. The dominant breakdown product of TCE degradation in the presence of Pd/MCM-41 was ethane. Minimal concentrations of intermediate degradation products were detected, if at all. This result suggests that TCE completely degrades to ethane before desorbing from the Pd/MCM-41 surface. It was shown that Pd/MCM-41 was more effective and had better longevity at treating inflow TCE compared to a lower cost substitute, Pd/sand. Unlike Pd/MCM-41, Ni/MCM-41 did not induce degradation of TCE. Column experiments using Ni-Pd/MCM-41 materials indicated that while the material does induce degradation of TCE, the Pd cannot be substituted for Ni on a 1:1 basis while still obtaining similar degradation results as Pd/MCM-41. Pd/MCM-41 was not able to substantially reduce initial concentrations of hexamethylphosphoramide (HMPA) in a batch experiment. A small reduction in the initial HMPA concentration was attributed to adsorption onto the Pd/MCM-41 surfaces rather than degradation of the compound. Several of the above-mentioned results suggest that MCM-41 and Pd/MCM-41 show great potential for being incorporated into water treatment technologies. Both the long term stability of the material in contact with deionized water and the longevity of a Pd/MCM-41 column in treating inflow TCE are very promising results with respect to applications in water treatment technologies. It is recommended that future work be pursued with this goal in mind.","abstract_html":"A research project was carried out to investigate several aspects of Mobil’s composition of matter #41 (MCM-41) pertaining to its potential application in water treatment technologies. The goal of the work was to lead to a recommendation of whether further work investigating this particular, potential application is warranted at the present time. A dissolution experiment indicated that Pd/MCM-41 is more stable in contact with deionized water at 25±0.1 degrees Celsius than purely siliceous MCM-41. Stability increases with increasing mass percent loading of Pd in the Pd/MCM-41 material. The increased stability was attributed to a reduction in Pd/MCM-41 surface areas relative to the parent MCM-41 material. The reduction in surface area is likely the result of partial or complete blocking of the MCM-41 mesopores by Pd centres. Ni/MCM-41 was less stable in contact with deionized water than MCM-41 and Pd/MCM-41. Both Ni and Pd impregnated MCM-41 exhibited enhanced stability relative to purely siliceous MCM-41 in 0.01 M NaCl solution. The stability enhancement was more pronounced for Pd/MCM-41. A long term dissolution experiment showed that MCM-41 retained its characteristic hexagonal mesopore structure and high surface area after 1,174 days of contact with deionized water. The ability of Pd/MCM-41 to absorb hydrogen was investigated in a series of experiments in pressure cells at 25±0.1 degrees Celsius and approximately 101.3 kPa. The Pd in Pd/MCM-41 was able to absorb 0.85±0.18 moles of hydrogen per mole of Pd present. This was a higher level of absorption than found in most other, published Pd-hydrogen investigations. It is proposed that enhanced uptake of hydrogen by Pd/MCM-41 may be the result of a higher proportion of surface and subsurface sites in the samples relative to other supported Pd materials. Batch and column trichloroethylene (TCE) degradation experiments indicated that Pd/MCM-41 has substantial longevity while degrading at least 91% of inflow TCE concentrations in hydrogen-saturated deionized water over 5,036 pore volumes. The average inflow TCE concentration was 4.94E-2 ± 4.87E-3 mmol/l with maximum and minimum concentrations of 7.24E-2 mmol/l and 2.63E-2 mmol/l, respectively. The dominant breakdown product of TCE degradation in the presence of Pd/MCM-41 was ethane. Minimal concentrations of intermediate degradation products were detected, if at all. This result suggests that TCE completely degrades to ethane before desorbing from the Pd/MCM-41 surface. It was shown that Pd/MCM-41 was more effective and had better longevity at treating inflow TCE compared to a lower cost substitute, Pd/sand. Unlike Pd/MCM-41, Ni/MCM-41 did not induce degradation of TCE. Column experiments using Ni-Pd/MCM-41 materials indicated that while the material does induce degradation of TCE, the Pd cannot be substituted for Ni on a 1:1 basis while still obtaining similar degradation results as Pd/MCM-41. Pd/MCM-41 was not able to substantially reduce initial concentrations of hexamethylphosphoramide (HMPA) in a batch experiment. A small reduction in the initial HMPA concentration was attributed to adsorption onto the Pd/MCM-41 surfaces rather than degradation of the compound. Several of the above-mentioned results suggest that MCM-41 and Pd/MCM-41 show great potential for being incorporated into water treatment technologies. Both the long term stability of the material in contact with deionized water and the longevity of a Pd/MCM-41 column in treating inflow TCE are very promising results with respect to applications in water treatment technologies. It is recommended that future work be pursued with this goal in mind.","abstract_has_math":false,"creators":["Guthrie, Colin Peter"],"institution":"University of Waterloo","degree_name":null,"degree_level":null,"degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":[],"committee_chairs":[],"committee_members":[],"year":2013,"date_issued":"2013-01-08T17:01:06Z","date_published":"2013-01-08T17:01:06Z","updated_at":"2026-11-19T10:50:02Z","subjects":["MCM-41","stability","hydrogen absorption","degradation"],"languages":["en"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":"http://hdl.handle.net/10012/7181","outbound_label":"Handle","outbound_source":"dc:identifier.uri","record_url":"http://hdl.handle.net/10012/7181","record_label":"Repository record","record_kind":"handle","record_source":"dc:identifier.uri","download_url":null,"download_label":null,"download_source":null,"access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://dspacemainprd01.lib.uwaterloo.ca/server/oai/request?verb=GetRecord&metadataPrefix=dim&identifier=oai%3Auwspace.uwaterloo.ca%3A10012%2F7181","prefix":"dim"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:creator","label":"Author","values":["Guthrie, Colin Peter"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date.accessioned","label":"Dc Date Accessioned","values":["2013-01-08T17:01:06Z"]},{"key":"dc:date.available","label":"Dc Date Available","values":["2013-01-08T17:01:06Z"]},{"key":"dc:date.issued","label":"Date","values":["2013-01-08T17:01:06Z"]},{"key":"dc:date.submitted","label":"Dc Date Submitted","values":["2012"]},{"key":"dc:publisher","label":"Institution","values":["University of Waterloo"]},{"key":"dc:type","label":"Dc Type","values":["Doctoral Thesis"]}]},{"id":"subjects_keywords","label":"Subjects and Keywords","entries":[{"key":"dc:subject","label":"Dc Subject","values":["MCM-41","stability","hydrogen absorption","degradation"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.iso","label":"Language (ISO)","values":["en"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["http://hdl.handle.net/10012/7181"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["A research project was carried out to investigate several aspects of Mobil’s composition of matter #41 (MCM-41) pertaining to its potential application in water treatment technologies. The goal of the work was to lead to a recommendation of whether further work investigating this particular, potential application is warranted at the present time. A dissolution experiment indicated that Pd/MCM-41 is more stable in contact with deionized water at 25±0.1 degrees Celsius than purely siliceous MCM-41. Stability increases with increasing mass percent loading of Pd in the Pd/MCM-41 material. The increased stability was attributed to a reduction in Pd/MCM-41 surface areas relative to the parent MCM-41 material. The reduction in surface area is likely the result of partial or complete blocking of the MCM-41 mesopores by Pd centres. Ni/MCM-41 was less stable in contact with deionized water than MCM-41 and Pd/MCM-41. Both Ni and Pd impregnated MCM-41 exhibited enhanced stability relative to purely siliceous MCM-41 in 0.01 M NaCl solution. The stability enhancement was more pronounced for Pd/MCM-41. A long term dissolution experiment showed that MCM-41 retained its characteristic hexagonal mesopore structure and high surface area after 1,174 days of contact with deionized water. The ability of Pd/MCM-41 to absorb hydrogen was investigated in a series of experiments in pressure cells at 25±0.1 degrees Celsius and approximately 101.3 kPa. The Pd in Pd/MCM-41 was able to absorb 0.85±0.18 moles of hydrogen per mole of Pd present. This was a higher level of absorption than found in most other, published Pd-hydrogen investigations. It is proposed that enhanced uptake of hydrogen by Pd/MCM-41 may be the result of a higher proportion of surface and subsurface sites in the samples relative to other supported Pd materials. Batch and column trichloroethylene (TCE) degradation experiments indicated that Pd/MCM-41 has substantial longevity while degrading at least 91% of inflow TCE concentrations in hydrogen-saturated deionized water over 5,036 pore volumes. The average inflow TCE concentration was 4.94E-2 ± 4.87E-3 mmol/l with maximum and minimum concentrations of 7.24E-2 mmol/l and 2.63E-2 mmol/l, respectively. The dominant breakdown product of TCE degradation in the presence of Pd/MCM-41 was ethane. Minimal concentrations of intermediate degradation products were detected, if at all. This result suggests that TCE completely degrades to ethane before desorbing from the Pd/MCM-41 surface. It was shown that Pd/MCM-41 was more effective and had better longevity at treating inflow TCE compared to a lower cost substitute, Pd/sand. Unlike Pd/MCM-41, Ni/MCM-41 did not induce degradation of TCE. Column experiments using Ni-Pd/MCM-41 materials indicated that while the material does induce degradation of TCE, the Pd cannot be substituted for Ni on a 1:1 basis while still obtaining similar degradation results as Pd/MCM-41. Pd/MCM-41 was not able to substantially reduce initial concentrations of hexamethylphosphoramide (HMPA) in a batch experiment. A small reduction in the initial HMPA concentration was attributed to adsorption onto the Pd/MCM-41 surfaces rather than degradation of the compound. Several of the above-mentioned results suggest that MCM-41 and Pd/MCM-41 show great potential for being incorporated into water treatment technologies. Both the long term stability of the material in contact with deionized water and the longevity of a Pd/MCM-41 column in treating inflow TCE are very promising results with respect to applications in water treatment technologies. It is recommended that future work be pursued with this goal in mind."]},{"key":"dc:title","label":"Title","values":["Behaviour of Mesoporous Silica (MCM-41) Supported Catalysts in Degradation Reactions"]},{"key":"others:access_status","label":"Others Access Status","values":["open.access"]}]}],"canonical_facts":{"dc:creator":["Guthrie, Colin Peter"],"dc:date.accessioned":["2013-01-08T17:01:06Z"],"dc:date.available":["2013-01-08T17:01:06Z"],"dc:date.issued":["2013-01-08T17:01:06Z"],"dc:date.submitted":["2012"],"dc:description.abstract":["A research project was carried out to investigate several aspects of Mobil’s composition of matter #41 (MCM-41) pertaining to its potential application in water treatment technologies. The goal of the work was to lead to a recommendation of whether further work investigating this particular, potential application is warranted at the present time. A dissolution experiment indicated that Pd/MCM-41 is more stable in contact with deionized water at 25±0.1 degrees Celsius than purely siliceous MCM-41. Stability increases with increasing mass percent loading of Pd in the Pd/MCM-41 material. The increased stability was attributed to a reduction in Pd/MCM-41 surface areas relative to the parent MCM-41 material. The reduction in surface area is likely the result of partial or complete blocking of the MCM-41 mesopores by Pd centres. Ni/MCM-41 was less stable in contact with deionized water than MCM-41 and Pd/MCM-41. Both Ni and Pd impregnated MCM-41 exhibited enhanced stability relative to purely siliceous MCM-41 in 0.01 M NaCl solution. The stability enhancement was more pronounced for Pd/MCM-41. A long term dissolution experiment showed that MCM-41 retained its characteristic hexagonal mesopore structure and high surface area after 1,174 days of contact with deionized water. The ability of Pd/MCM-41 to absorb hydrogen was investigated in a series of experiments in pressure cells at 25±0.1 degrees Celsius and approximately 101.3 kPa. The Pd in Pd/MCM-41 was able to absorb 0.85±0.18 moles of hydrogen per mole of Pd present. This was a higher level of absorption than found in most other, published Pd-hydrogen investigations. It is proposed that enhanced uptake of hydrogen by Pd/MCM-41 may be the result of a higher proportion of surface and subsurface sites in the samples relative to other supported Pd materials. Batch and column trichloroethylene (TCE) degradation experiments indicated that Pd/MCM-41 has substantial longevity while degrading at least 91% of inflow TCE concentrations in hydrogen-saturated deionized water over 5,036 pore volumes. The average inflow TCE concentration was 4.94E-2 ± 4.87E-3 mmol/l with maximum and minimum concentrations of 7.24E-2 mmol/l and 2.63E-2 mmol/l, respectively. The dominant breakdown product of TCE degradation in the presence of Pd/MCM-41 was ethane. Minimal concentrations of intermediate degradation products were detected, if at all. This result suggests that TCE completely degrades to ethane before desorbing from the Pd/MCM-41 surface. It was shown that Pd/MCM-41 was more effective and had better longevity at treating inflow TCE compared to a lower cost substitute, Pd/sand. Unlike Pd/MCM-41, Ni/MCM-41 did not induce degradation of TCE. Column experiments using Ni-Pd/MCM-41 materials indicated that while the material does induce degradation of TCE, the Pd cannot be substituted for Ni on a 1:1 basis while still obtaining similar degradation results as Pd/MCM-41. Pd/MCM-41 was not able to substantially reduce initial concentrations of hexamethylphosphoramide (HMPA) in a batch experiment. A small reduction in the initial HMPA concentration was attributed to adsorption onto the Pd/MCM-41 surfaces rather than degradation of the compound. Several of the above-mentioned results suggest that MCM-41 and Pd/MCM-41 show great potential for being incorporated into water treatment technologies. Both the long term stability of the material in contact with deionized water and the longevity of a Pd/MCM-41 column in treating inflow TCE are very promising results with respect to applications in water treatment technologies. It is recommended that future work be pursued with this goal in mind."],"dc:identifier.uri":["http://hdl.handle.net/10012/7181"],"dc:language.iso":["en"],"dc:publisher":["University of Waterloo"],"dc:subject":["MCM-41","stability","hydrogen absorption","degradation"],"dc:title":["Behaviour of Mesoporous Silica (MCM-41) Supported Catalysts in Degradation Reactions"],"dc:type":["Doctoral Thesis"],"others:access_status":["open.access"]},"updated_at":"2026-11-19T10:50:02Z"}