{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:17446"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:17446","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Relationship between Microstructure, Durability and Performance of CEM X Composite Cements","abstract":"Cement production is a major contributor to anthropogenic CO2 emissions. Composite slag cement is one way of reducing the clinker factor, and hence emissions. Synergies between limestone and slag have been suggested to enhance the performance of such cement. The synergistic effect on mechanical performance has been ascribed to the carboalumination formation, which in turn prevents the conversion of ettringite to mono sulphoaluminate. Whilst the benefits of the synergy are documented, causation factors are not fully understood. In order to maximise the synergy, a clear understanding of the relationship between composition and the carboalumination-ettringite balance and how this impacts on performance is essential. Consequently, this study focused on the kinetics of reaction, microstructure and the implications on strength development and the freeze-thaw durability. The QXRD/PONKCS method proposed elsewhere has been extended to monitor the residual slag contents in ternary blended systems. The slag phase was modelled from the x-ray diffraction pattern of a 100 % slag specimen. The model was then calibrated on a 50:50 mixture of slag and corundum using the internal standard method. The measurement accuracy was found to be ± 2 % following implementation of the calibrated slag phase on simplified slag-corundum mixes of varying proportions. In hydrated cement systems, however, the accuracy established from the comparison between the results from QXRD/PONKCS and SEM/IA analysis was ± 6 %. The investigated hydration stopping methods except freeze-drying had minimal impact on the results as long as the mass attenuation coefficient (MAC) was accurately quantified. For implementing the QXRD/PONKCS method, freshly ground non-hydration stopped sample preparation is recommended. This method presented the least challenge in calculating the MAC and also preserve the other hydrates particularly the AFt/AFm phases. However, if hydration stopping cannot be avoided, a double solvent exchange regime using isopropanol and diethyl ether is recommended. The residual slag content is overestimated from freeze-dried samples. Multiple techniques including the QXRD/PONKCS method, SEM/IA, isothermal conduction calorimetry, chemical shrinkage and thermal analysis were subsequently used to investigate the kinetics of hydration. These revealed that limestone accelerates slag and clinker hydration. Alite hydration is accelerated by the supplementary cementitious materials including slag and quartz. However, while belite hydration is retarded in the binary slag mix, this is not the case in limestone ternary blends. Calcium carbonate also reacts with additionally dissolved aluminates instead of the latter converting ettringite to mono sulphoaluminate. Therefore, the synergy between limestone and slag is not only due to preserved ettringite but the additional hydrates and pore structure modification. The carboaluminate content is higher in the presence of limestone but the home to mono carboaluminate balance shifts with the limestone content. The aluminates available for incorporation into other hydrates and in the pore solution are lowered by carboaluminate formation. The pore structure and pore solution chemistry were analysed in order to further investigate the mechanisms for the accelerated dissolution of slag and the major clinker phases. The overall pore volumes as measured by MIP were similar in the slag containing mixes with or without limestone. Evaluation of the free water content at the end of experiment also indicated excess free water thus indicating that the pore structure and capillary pore water are not the limiting factors for slag hydration in the investigated mixes. The identified drivers behind the role of limestone in the synergy are the nucleation and dilution effects in the case of clinker, while for slag hydration pore solution effects are important. The incorporation of alumina into carboaluminates and C-S-H lowers the alumina in the pore solution and consequently promote slag dissolution. The freeze-thaw resistance of the ternary blends at the investigated 0.5 water/binder ratio is low compared to the CEM I 42.5 R concrete. Decalcification through carbonation during conditioning and leaching during freeze-thaw is identified to be the dominant microstructural difference between degraded and non-degraded samples. A chemo-mechanical degradation mechanism, which is similar to the glue-spall mechanism, is hypothesised for surface scaling during freeze-thaw. By this, freeze-thaw damage in concrete is caused by decalcification and spalling of successive layers under induced stresses of ice growth.","abstract_html":"Cement production is a major contributor to anthropogenic CO2 emissions. Composite slag cement is one way of reducing the clinker factor, and hence emissions. Synergies between limestone and slag have been suggested to enhance the performance of such cement. The synergistic effect on mechanical performance has been ascribed to the carboalumination formation, which in turn prevents the conversion of ettringite to mono sulphoaluminate. Whilst the benefits of the synergy are documented, causation factors are not fully understood. In order to maximise the synergy, a clear understanding of the relationship between composition and the carboalumination-ettringite balance and how this impacts on performance is essential. Consequently, this study focused on the kinetics of reaction, microstructure and the implications on strength development and the freeze-thaw durability. The QXRD/PONKCS method proposed elsewhere has been extended to monitor the residual slag contents in ternary blended systems. The slag phase was modelled from the x-ray diffraction pattern of a 100 % slag specimen. The model was then calibrated on a 50:50 mixture of slag and corundum using the internal standard method. The measurement accuracy was found to be ± 2 % following implementation of the calibrated slag phase on simplified slag-corundum mixes of varying proportions. In hydrated cement systems, however, the accuracy established from the comparison between the results from QXRD/PONKCS and SEM/IA analysis was ± 6 %. The investigated hydration stopping methods except freeze-drying had minimal impact on the results as long as the mass attenuation coefficient (MAC) was accurately quantified. For implementing the QXRD/PONKCS method, freshly ground non-hydration stopped sample preparation is recommended. This method presented the least challenge in calculating the MAC and also preserve the other hydrates particularly the AFt/AFm phases. However, if hydration stopping cannot be avoided, a double solvent exchange regime using isopropanol and diethyl ether is recommended. The residual slag content is overestimated from freeze-dried samples. Multiple techniques including the QXRD/PONKCS method, SEM/IA, isothermal conduction calorimetry, chemical shrinkage and thermal analysis were subsequently used to investigate the kinetics of hydration. These revealed that limestone accelerates slag and clinker hydration. Alite hydration is accelerated by the supplementary cementitious materials including slag and quartz. However, while belite hydration is retarded in the binary slag mix, this is not the case in limestone ternary blends. Calcium carbonate also reacts with additionally dissolved aluminates instead of the latter converting ettringite to mono sulphoaluminate. Therefore, the synergy between limestone and slag is not only due to preserved ettringite but the additional hydrates and pore structure modification. The carboaluminate content is higher in the presence of limestone but the home to mono carboaluminate balance shifts with the limestone content. The aluminates available for incorporation into other hydrates and in the pore solution are lowered by carboaluminate formation. The pore structure and pore solution chemistry were analysed in order to further investigate the mechanisms for the accelerated dissolution of slag and the major clinker phases. The overall pore volumes as measured by MIP were similar in the slag containing mixes with or without limestone. Evaluation of the free water content at the end of experiment also indicated excess free water thus indicating that the pore structure and capillary pore water are not the limiting factors for slag hydration in the investigated mixes. The identified drivers behind the role of limestone in the synergy are the nucleation and dilution effects in the case of clinker, while for slag hydration pore solution effects are important. The incorporation of alumina into carboaluminates and C-S-H lowers the alumina in the pore solution and consequently promote slag dissolution. The freeze-thaw resistance of the ternary blends at the investigated 0.5 water/binder ratio is low compared to the CEM I 42.5 R concrete. Decalcification through carbonation during conditioning and leaching during freeze-thaw is identified to be the dominant microstructural difference between degraded and non-degraded samples. A chemo-mechanical degradation mechanism, which is similar to the glue-spall mechanism, is hypothesised for surface scaling during freeze-thaw. By this, freeze-thaw damage in concrete is caused by decalcification and spalling of successive layers under induced stresses of ice growth.","abstract_has_math":false,"creators":["Adu-Amankwah, Samuel"],"institution":"University of Leeds","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Black, Leon"],"committee_chairs":[],"committee_members":[],"year":2016,"date_issued":"2016-10","date_published":"2016-10","updated_at":"2026-11-18T22:21:38Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.714270"],"render_values":[{"text":"uk.bl.ethos.714270","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/17446/1/The%20Relationship%20between%20composition%20microstructure%20and%20performance%20of%20composite%20cements-Corrected.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A17446","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Black, Leon"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["University of Leeds","Heidelberg Technology Centre"]},{"key":"dc:creator","label":"Author","values":["Adu-Amankwah, Samuel"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2016-10-31"]},{"key":"dc:date.issued","label":"Date","values":["2016-10"]},{"key":"dc:publisher.commercial","label":"Dc Publisher Commercial","values":["University of Leeds"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Faculty of Engineering (Leeds)","School of Civil Engineering (Leeds)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Leeds"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/17446/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["List of References [1] J.S. Damtoft, J. Lukasik, D. Herfort, D. Sorrentino, E.M. Gartner, Sustainable development and climate change initiatives, Cement and Concrete Research, 38 (2008) 115-127. [2] ECOBA, European Coal Ash Unitlisation, in, 2016. [3] J.A. Ober, Mineral commodity summaries 2016, in, US Geological Survey, 2016. [4] V. Bonavetti, H. Donza, V. Rahhal, E. Irassar, Influence of initial curing on the properties of concrete containing limestone blended cement, Cement and Concrete Research, 30 (2000) 703-708. [5] R. Hooton, M. Nokken, M. Thomas, Portland-limestone cement: state-of-the-art report and gap analysis for CSA A 3000, Cement Association of Canada University of Toronto, (2007). [6] P.D. Tennis, M.D.A. Thomas, W.J. Weiss, State-of-the-Art Report on Use of Limestone in Cements at Levels of up to 15%, in, Portland Cement Association, Skokie, Illinois, 2011, pp. 78. [7] K. De Weerdt, M. Ben Haha, G. Le Saout, K.O. Kjellsen, H. Justnes, B. Lothenbach, Hydration mechanisms of ternary Portland cements containing limestone powder and fly ash, Cement and Concrete Research, 41 (2011) 279-291. [8] G. Menéndez, V. Bonavetti, E.F. Irassar, Strength development of ternary blended cement with limestone filler and blast-furnace slag, Cement and Concrete Composites, 25 (2003) 61-67. [9] M. Moesgaard, S.L. Poulsen, D. Herfort, M. Steenberg, L.K. Kirkegaard, J. Skibsted, Y. Yue, Hydration of Blended Portland Cements Containing Calcium-Aluminosilicate Glass Powder and Limestone, Journal of the American Ceramic Society, 95 (2012) 403–409. [10] B. Lothenbach, K. Scrivener, R.D. Hooton, Supplementary cementitious materials, Cement and Concrete Research, 41 (2011) 1244-1256. [11] X. Wu, W. Jiang, D.M. Roy, Early activation and properties of slag cement, Cement and Concrete Research, 20 (1990) 961-974. [12] J.I. Escalante, L.Y. Gómez, K.K. Johal, G. Mendoza, H. Mancha, J. Méndez, Reactivity of blast-furnace slag in Portland cement blends hydrated under different conditions, Cement and Concrete Research, 31 (2001) 1403-1409. [13] J. Cailetti, A.M. Soliman, M.L. Nehdi, Effects of nano- and micro-limestone addition on early-age properties of ultra-high-performance concrete, Materials and Structures, 46 (2013) 881-898. [14] S. Hoshino, K. Yamada, H. Hirao, XRD/Rietveld analysis of the hydration and strength development of slag and limestone blened cement, Advanced Concrete Technology, 4 (2006) 357-367. [15] S. Ogawa, T. Nozaki, K. Yamada, H. Hirao, R.D. Hooton, Improvement on sulfate resistance of blended cement with high alumina slag, Cement and Concrete Research, 42 (2012) 244-251. [16] S. Tsivilis, E. Chaniotakis, E. Badogiannis, G. Pahoulas, A. Ilias, A study on the parameters affecting the properties of Portland limestone cements, Cement and Concrete Composites, 21 (1999) 107-116. [17] B. Lothenbach, G. Le Saout, E. Gallucci, K. Scrivener, Influence of limestone on the hydration of Portland cements, Cement and Concrete Research, 38 (2008) 848-860. [18] M. Moesgaard, D. Herfort, M. Steenberg, L.F. Kirkegaard, Y. Yue, Physical performances of blended cements containing calcium aluminosilicate glass powder and limestone, Cement and Concrete Research, 41 (2011) 359-364. [19] A.M. Ramezanianpour, R.D. Hooton, Sulfate resistance of Portland-limestone cements in combination with supplementary cementitious materials, Materials and Structures, 46 (2012) 1061-1073 [20] T. Schmidt, B. Lothenbach, M. Romer, J. Neuenschwander, K. Scrivener, Physical and microstructural aspects of sulfate attack on ordinary and limestone blended Portland cements, Cement and Concrete Research, 39 (2009) 1111-1121. [21] K.u. Githachuri, M.G. Alexander, Durability performance potential and strength of blended Portland limestone cement concrete, Cement and Concrete Composites, 39 (2013) 115-121. [22] B. Persson, Internal frost resistance and salt frost scaling of self-compacting concrete, Cement and Concrete Research, 33 (2003) 373-379. [23] S. Grzeszczyk, P. Podkowa, The Effect of Limestone Filler on the Properties of Self Compacting Concrete, ANNUAL TRANSACTIONS OF THE NORDIC RHEOLOGY SOCIETY, , VOL. 17 (2009). [24] R.K. Dhir, M.C. Limbachiya, M.J. Macarthy, A. Chaipanich, Evaluation of Portland limestone cements for use in concrete construction, Materials and Structures, 40 (2007) 459 - 473. [25] J. Stark, H.M. Ludwig, Freeze-deicing salt resistance of concretes containing cement rich in slag, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop, E & FN SPON, University of Essen, 1997, pp. 123-138. [26] B. Espion, B. Lebon, O. Germain, A. Hellebois, Characterisation of new ternary cements with reduced clinker content in: K. Sakai (Ed.) Proceedings of the First International Conference on Concrete Sustainability, Tokyo, Japan, 2013, pp. 145 - 152. [27] M. Collepardi, S. Collepardi, J.J. Ogoumah Olagot, E. Simonelli, The Influence of Slag and Fly Ash on the Carbonation, in: V.M. Malhotra (Ed.) Eighth CANMET/ACI International Conference on Fly Ash, Silica Fume, Slag, and Natural Pozzolans in Concrete 2004. [28] M. Ben Haha, K. De Weerdt, B. Lothenbach, Quantification of the degree of reaction of fly ash, Cement and Concrete Research, 40 (2010) 1620-1629. [29] V. Kocaba, E. Gallucci, K.L. Scrivener, Methods for determination of degree of reaction of slag in blended cement pastes, Cement and Concrete Research, 42 (2012) 511-525. [30] K. Luke, F.P. Glasser, Selective dissolution of hydrated blast furnace slag cements, Cement and Concrete Research, 17 (1987) 273-282. [31] M. Whittaker, M. Zajac, M. Ben Haha, F. Bullergahn, L. Black, The role of the alumina content of slag, plus the presence of additional sulfate on the hydration and microstructure of Portland cement-slag blends, Cement and Concrete Research, 66 (2014) 91-101. [32] N.V.Y. Scarlett, I.C. Madsen, Quantification of phases with partial or no known crystal structures, Powder Diffraction, 21 (2006) 278-284. [33] R. Snellings, A. Salze, K.L. Scrivener, Use of X-ray diffraction to quantify amorphous supplementary cementitious materials in anhydrous and hydrated blended cements, Cement and Concrete Research, 64 (2014) 89-98. [34] J. Marchand, Y. Maltais, Y. Machabee, C. TAlbot, M. Pigeon, Effects of fly ash on microstructure and deicer salt scaling resistance of concrete, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop, University of Essen, 1997, pp. 11 - 20. [35] J.J. Valenza Ii, G.W. Scherer, A review of salt scaling: II. Mechanisms, Cement and Concrete Research, 37 (2007) 1022-1034. [36] J.J. Valenza, G.W. Scherer, A review of salt scaling: I. Phenomenology, Cement and Concrete Research, 37 (2007) 1007-1021. [37] T.C. Powers, A Working Hypothesis for Further Studies of Frost Resistance of Concrete, ACI Journal Proceedings, 41 (1945) 245-272. [38] T.C. Powers, R.A. Helmuth, Theory of volume changes in hardened Portland cement paste during freezing, Highway Research Board, 32 (1953). [39] G.W. Scherer, Crystallization in pores, Cement and Concrete Research, 29 (1999) 1347-1358. [40] G.W. Scherer, J. Valenza, Mechanisms of frost damage, Materials science of concrete, 7 (2005) 209-246. [41] P.-w. Gao, S.-x. Wu, P.-h. Lin, Z.-r. Wu, M.-s. Tang, The characteristics of air void and frost resistance of RCC with fly ash and expansive agent, Construction and Building Materials, 20 (2006) 586-590. [42] G.-F. Peng, Q. Ma, H.-M. Hu, R. Gao, Q.-F. Yao, Y.-F. Liu, The effects of air entrainment and pozzolans on frost resistance of 50–60&#xa0;MPa grade concrete, Construction and Building Materials, 21 (2007) 1034-1039. [43] K. Fridh, Internal frost damage in concrete - experimental studies of destruction mechanisms, in: Division of Building Materials, University of Lund, 2005. [44] J. Deja, Freezing and de-icing salt resistance of blast furnace slag concretes, Cement and Concrete Composites, 25 (2003) 357-361. [45] D.J. Janssen, M.B. Snyder, Resistance of concrete to freezing and thawing, 1994. [46] K.L. Scrivener, Backscattered electron imaging of cementitious microstructures: understanding and quantification, Cement and Concrete Composites, 26 (2004) 935-945. [47] R.J. Detwiler, B.J. Dalgleish, R.B. Williamson, Assessing the durability of concrete in freezing and thawing, ACI Materials Journal, 86 (1989) 29-35. [48] M. Tang, Y. Tian, X.B. Mu, M. Jiang, The Pore Fractal Characteristics of Concrete Materials under Salt Freezing Conditions in Cold Area, Advanced Materials Research, 233 - 235 (2011) 2522 - 2527. [49] N.V. Scarlett, I.C. Madsen, Current state of quantitative phase analysis, in: Accuracy in Powder Diffraction, APD-IV, 2013. [50] E. Gartner, Industrially interesting approaches to “low-CO2” cements, Cement and Concrete Research, 34 (2004) 1489-1498. [51] E. Berodier, K. Scrivener, Understanding the filler effect on the nucleation and growth of C-S-H, Journal of the American Ceramic Society, 97 (2014) 3764-3773. [52] F. Deschner, F. Winnefeld, B. Lothenbach, S. Seufert, P. Schwesig, S. Dittrich, F. Goetz-Neunhoeffer, J. Neubauer, Hydration of Portland cement with high replacement by siliceous fly ash, Cement and Concrete Research, 42 (2012) 1389-1400. [53] K.L. Scrivener, P. Juilland, P.J.M. Monteiro, Advances in understanding hydration of Portland cement, Cement and Concrete Research, 78, Part A (2015) 38-56. [54] E. Berodier, K. Scrivener, Evolution of pore structure in blended systems, Cement and Concrete Research, 73 (2015) 25-35. [55] B. Lothenbach, G. Le Saout, M. Ben Haha, R. Figi, E. Wieland, Hydration of a low-alkali CEM III/B–SiO2 cement (LAC), Cement and Concrete Research, 42 (2012) 410-423. [56] CEMBUREAU, Environmental benefits of using alternative fuels in cement production: A life-cycle approach, in, The European Cement Association, 2010. [57] G. Habert, C. Billard, P. Rossi, C. Chen, N. Roussel, Cement production technology improvement compared to factor 4 objectives, Cement and Concrete Research, 40 (2010) 820-826. [58] G.P. Hammond, C.I. Jones, Embodied energy and carbon in construction materials, Proc Institution of Civil Engineers: Energy, (2008). [59] Ernst Worrell, Lynn Price, Nathan Martin, Chris Hendriks, L.O. Meida, Carbon dioxide emissions from the global cement industry, Annual Review of Energy and the Environment, 26 (2001) 303-329. [60] P. Mehta, H. Meryman, Tools for Reducing Carbon Emissions Due to Cement Consumption, Structure Magazine, (2009) 11-15. [61] P. Purnell, L. Black, Embodied carbon dioxide in concrete: Variation with common mix design parameters, Cement and Concrete Research, 42 (2012) 874-877. [62] J.H. Sharp, E.M. Gartner, D.E. Macphee, Novel cement systems (sustainability). Session 2 of the Fred Glasser Cement Science Symposium, Advances in Cement Research, 22 (2010) 195-202. [63] A. Palomo, M.W. Grutzeck, M.T. Blanco, Alkali-activated fly ashes: A cement for the future, Cement and Concrete Research, 29 (1999) 1323-1329. [64] F. Winnefeld, B. Lothenbach, Hydration of calcium sulfoaluminate cements — Experimental findings and thermodynamic modelling, Cement and Concrete Research, 40 (2010) 1239-1247. [65] Y. Li, B. Chen, Factors that affect the properties of magnesium phosphate cement, Construction and Building Materials, 47 (2013) 977-983. [66] J.W. Phair, Green chemistry for sustainable cement production and use, Green Chemistry, 8 (2006) 763-780. [67] K. Scrivener, B. Lothenbach, N. De Belie, E. Gruyaert, J. Skibsted, R. Snellings, A. Vollpracht, TC 238-SCM: hydration and microstructure of concrete with SCMs, Materials and Structures, 48 (2015) 835-862. [68] E. Badogiannis, S. Tsivilis, Exploitation of poor Greek kaolins: Durability of metakaolin concrete, Cement and Concrete Composites, 31 (2009) 128-133. [69] T.W. Cheng, J.P. Chiu, Fire-resistant geopolymer produced by granulated blast furnace slag, Minerals Engineering, 16 (2003) 205-210. [70] K.L. Scrivener, J.-L. Cabiron, R. Letourneux, High-performance concretes from calcium aluminate cements, Cement and Concrete Research, 29 (1999) 1215-1223. [71] J. Bensted, Calcium aluminate cements, in: J.Bensted, P.Barnes (Eds.) Structure and Performance of Cements, SPON Press, 2002, pp. 114-138. [72] K. Scrivener, Calcium aluminate cements, in: J. Newman, B.S. Choo (Eds.) Advanced Concrete Technology 1: Constituent Materials, Butterworth-Heinemann, 2003, pp. 2/1-2/29. [73] F.P. Glasser, L. Zhang, High-performance cement matrices based on calcium sulfoaluminate–belite compositions, Cement and Concrete Research, 31 (2001) 1881-1886. [74] K. Quillin, Performance of belite–sulfoaluminate cements, Cement and Concrete Research, 31 (2001) 1341-1349. [75] J.L. Provis, Geopolymers and other alkali activated materials: why, how, and what?, Materials and Structures, 47 (2014) 11-25. [76] S.A. Bernal, J.L. Provis, R.J. Myers, R. San Nicolas, J.S. van Deventer, Role of carbonates in the chemical evolution of sodium carbonate-activated slag binders, Materials and Structures, 48 (2015) 517-529. [77] P. Duxson, A. Fernández-Jiménez, J.L. Provis, G.C. Lukey, A. Palomo, J.S.J. van Deventer, Geopolymer technology: the current state of the art, Journal of Materials Science, 42 (2007) 2917-2933. [78] A. Fernández-Jiménez, A. Palomo, Composition and microstructure of alkali activated fly ash binder: Effect of the activator, Cement and Concrete Research, 35 (2005) 1984-1992. [79] A. Fernández-Jiménez, A. Palomo, M. Criado, Microstructure development of alkali-activated fly ash cement: a descriptive model, Cement and Concrete Research, 35 (2005) 1204-1209. [80] B.C. McLellan, R.P. Williams, J. Lay, A. Van Riessen, G.D. Corder, Costs and carbon emissions for geopolymer pastes in comparison to ordinary Portland cement, Journal of Cleaner Production, 19 (2011) 1080-1090. [81] D.N. Huntzinger, T.D. Eatmon, A life-cycle assessment of Portland cement manufacturing: comparing the traditional process with alternative technologies, Journal of Cleaner Production, 17 (2009) 668-675. [82] H.F.W. Taylor, Nanostructure of CSH: Current status, Advanced Cement Based Materials, 1 (1993) 38-46. [83] H.F.W. Taylor, Cement Chemistry, 2nd ed., Thomas Telford, 1997. [84] N.L. Thomas, D.D. Double, The hydration of Portland cement, C3S and C2S in the presence of a calcium complexing admixture (EDTA), Cement and Concrete Research, 13 (1983) 391-400. [85] P. Barret, D. Ménétrier, Filter dissolution of C3S as a function of the lime concentration in a limited amount of lime water, Cement and Concrete Research, 10 (1980) 521-534. [86] J.W. Bullard, H.M. Jennings, R.A. Livingston, A. Nonat, G.W. Scherer, J.S. Schweitzer, K.L. Scrivener, J.J. Thomas, Mechanisms of cement hydration, Cement and Concrete Research, 41 (2011) 1208-1223. [87] H.F.W. Taylor, P. Barret, P.W. Brown, D.D. Double, G. Frohnsdorff, V. Johansen, D. Ménétrier-Sorrentino, I. Odler, L.J. Parrott, J.M. Pommersheim, M. Regourd, J.F. Young, The hydration of tricalcium silicate, Matériaux et Construction 17 (1984) 457-468 [88] S. Mindess, J.F. Young, D. Darwin, Concrete, Prentice Hall PTR, 2003. [89] D. Stephan, S. Wistuba, Crystal structure refinement and hydration behaviour of 3CaO·SiO2 solid solutions with MgO, Al2O3 and Fe2O3, Journal of the European Ceramic Society, 26 (2006) 141-148. [90] M. Bigare, A. Guinier, C. Mazieres, M. Regourd, N. YannaquisS, W. Eysbl, T. HahnA, E. Woermann, Polymorphism of Tricalcium Silicate and Its Solid Solutions, Journal of the American Ceramic Society, 50 (1967) 609-619. [91] S. Ma, W. Zhou, S. Wang, W. Li, X. Shen, Polymorph transformation kinetics of Ca3SiO5 with MgO, Phase Transitions, 88 (2015) 888-896. [92] M.-N. de Noirfontaine, M. Courtial, F. Dunstetter, G. Gasecki, M. Signes-Frehel, Tricalcium silicate Ca3SiO5 superstructure analysis: a route towards the structure of the M1 polymorph, in: Zeitschrift für Kristallographie Crystalline Materials, 2012, pp. 102. [93] F. Dunstetter, M.N. de Noirfontaine, M. Courtial, Polymorphism of tricalcium silicate, the major compound of Portland cement clinker: 1. Structural data: review and unified analysis, Cement and Concrete Research, 36 (2006) 39-53. [94] I. Odler, Hydration, Setting and Hardening of Portland Cement in: Lea’s Chemistry of Cement&Concrete, Butterworth Heinemann, Oxford, 2001, pp. 241. [95] S. Abdul-Maula, I. Odler, Structure and properties of tricalcium silicate doped with MgO, Al 2 O 3 and Fe 2 O 3, in: Proc Br Ceram Soc, 1984, pp. 83. [96] D. Stephan, S.N. Dikoundou, G. Raudaschl-Sieber, Hydration characteristics and hydration products of tricalcium silicate doped with a combination of MgO, Al2O3 and Fe2O3, Thermochimica Acta, 472 (2008) 64-73. [97] G.L. Valenti, V. Sabatelli, B. Marchese, Hydration kinetics of tricalcium silicate solid solutions at early ages, Cement and Concrete Research, 8 (1978) 61-72. [98] I.a. Odler, S. Abdul-Maula, Polymorphism and Hydration of Tricalcium Silicate Doped With ZnO, Journal of the American Ceramic Society, 66 (1983) 1-4. [99] H.R. Stewart, J.E. Bailey, Microstructural studies of the hydration products of three tricalcium silicate polymorphs, Journal of Materials Science, 18 (1983) 3686-3694. [100] A. Bazzoni, S. Ma, Q. Wang, X. Shen, M. Cantoni, K.L. Scrivener, The Effect of Magnesium and Zinc Ions on the Hydration Kinetics of C3S, Journal of the American Ceramic Society, 97 (2014) 3684-3693. [101] T. Staněk, P. Sulovský, The influence of the alite polymorphism on the strength of the Portland cement, Cement and Concrete Research, 32 (2002) 1169-1175. [102] L. Fernandez, C. Alonso, A. Hidalgo, C. Andrade, The role of magnesium during the hydration of C3S and CSH formation. Scanning electron microscopy and mid-infrared studies, Advances in cement research, 17 (2005) 9-21. [103] I.G. Richardson, G.W. Groves, Microstructure and microanalysis of hardened ordinary Portland cement pastes, Journal of Materials Science, 28 (1993) 265-277. [104] I.G. Richardson, A.R. Brough, R. Brydson, G.W. Groves, C.M. Dobson, Location of Aluminum in Substituted Calcium Silicate Hydrate (C-S-H) Gels as Determined by 29Si and 27Al NMR and EELS, Journal of the American Ceramic Society, 76 (1993) 2285 - 2286. [105] C. Tashiro, S. Tatibana, Bond strength between C3S paste and iron, copper or zinc wire and microstructure of interface, Cement and Concrete Research, 13 (1983) 377-382. [106] D. Jansen, S.T. Bergold, F. Goetz-Neunhoeffer, J. Neubauer, The hydration of alite: a time-resolved quantitative X-ray diffraction approach using the G-factor method compared with heat release, J Appl Cryst, 44 (2011) 895-901. [107] D. Jansen, F. Goetz-Neunhoeffer, B. Lothenbach, J. Neubauer, The early hydration of Ordinary Portland Cement (OPC): An approach comparing measured heat flow with calculated heat flow from QXRD, Cement and Concrete Research, 42 (2012) 134-138. [108] J.B. Ings, P.W. Brown, G. Frohnsdorff, Early hydration of large single crystals of tricalcium silicate, Cement and Concrete Research, 13 (1983) 843-848. [109] J.J. Thomas, H.M. Jennings, J.J. Chen, Influence of Nucleation Seeding on the Hydration Mechanisms of Tricalcium Silicate and Cement, The Journal of Physical Chemistry, 113 (2009) 4327-4334. [110] A. Comotti, G. Castaldi, C. Gilioli, G. Torri, P. Sozzani, Step-by-step observation of the hydration of C3S by magic-angle spinning 29Si nuclear magnetic resonance: the masking effect of D2O, Journal of Materials Science, 29 (1994) 6427-6433. [111] J.J. Thomas, S.A. FitzGerald, D.A. Neumann, R.A. Livingston, State of Water in Hydrating Tricalcium Silicate and Portland Cement Pastes as Measured by Quasi-Elastic Neutron Scattering, Journal of the American Ceramic Society, 84 (2001) 1811-1816. [112] E. Pustovgar, R.P. Sangodkar, A.S. Andreev, M. Palacios, B.F. Chmelka, R.J. Flatt, J.-B. d/'Espinose de Lacaillerie, Understanding silicate hydration from quantitative analyses of hydrating tricalcium silicates, Nat Commun, 7 (2016). [113] E.M. Gartner, Hydration mechanisms I, American Ceramic Society, 1 (1989) 95-125. [114] P. Juilland, E. Gallucci, R. Flatt, K. Scrivener, Dissolution theory applied to the induction period in alite hydration, Cement and Concrete Research, 40 (2010) 831-844. [115] A. Nonat, The structure and stoichiometry of C-S-H, Cement and Concrete Research, 34 (2004) 1521-1528. [116] E.M. Gartner, H.M. Jennings, Thermodynamics of calcium silicate hydrates and their solutions, J Am Ceram Soc 80 (1987) 743–749. [117] H.N. Stein, J.M. Stevels, Influence of silica on the hydration of 3 CaO,SiO2, Journal of Applied Chemistry, 14 (1964) 338-346. [118] H.M. Jennings, P.L. Pratt, An experimental argument for the existence of a protective membrane surrounding portland cement during the induction period, Cement and Concrete Research, 9 (1979) 501-506. [119] S. Garrault, T. Behr, A. Nonat, Formation of the C−S−H Layer during Early Hydration of Tricalcium Silicate Grains with Different Sizes, The Journal of Physical Chemistry B, 110 (2006) 270-275. [120] S. Garrault, E. Finot, E. Lesniewska, A. Nonat, Study of C-S-H growth on C3S surface during its early hydration, Materials and Structures, 38 (2005) 435-442. [121] F. Tzschichholz, H. Zanni, Global hydration kinetics of tricalcium silicate cement, Physical Review E, 64 (2001) 016115. [122] A. Kumar, S. Bishnoi, K.L. Scrivener, Modelling early age hydration kinetics of alite, Cement and Concrete Research, 42 (2012) 903-918. [123] A.K. Chatterjee, High belite cements—Present status and future technological options: Part I, Cement and Concrete Research, 26 (1996) 1213-1225. [124] J.G. Jang, H.K. Lee, Microstructural densification and CO2 uptake promoted by the carbonation curing of belite-rich Portland cement, Cement and Concrete Research, 82 (2016) 50-57. [125] T. Link, F. Bellmann, H.M. Ludwig, M. Ben Haha, Reactivity and phase composition of Ca2SiO4 binders made by annealing of alpha-dicalcium silicate hydrate, Cement and Concrete Research, 67 (2015) 131-137. [126] S.N. Ghosh, P.B. Rao, A.K. Paul, K. Raina, The chemistry of dicalcium silicate mineral, Journal of Materials Science, 14 (1979) 1554-1566. [127] Y.J. Kim, I. Nettleship, W.M. Kriven, Phase Transformations in Dicalcium Silicate: II, TEM Studies of Crystallography, Microstructure, and Mechanisms, Journal of the American Ceramic Society, 75 (1992) 2407-2419. [128] H.-M. Ludwig, W. Zhang, Research review of cement clinker chemistry, Cement and Concrete Research, 78, Part A (2015) 24-37. [129] H. Ishida, S. Yamazaki, K. Sasaki, Y. Okada, T. Mitsuda, α-Dicalcium Silicate Hydrate: Preparation, Decomposed Phase, and Its Hydration, Journal of the American Ceramic Society, 76 (1993) 1707-1712. [130] K. Fukuda, N. Wakamatsu, S. Ito, Improvement in Hydration Reactivity of α-Phase Belite by Remelting Reaction, Journal of the American Ceramic Society, 84 (2001) 639-641. [131] K. Morsli, Á.G. De La Torre, S. Stöber, A.J.M. Cuberos, M. Zahir, M.A.G. Aranda, Quantitative Phase Analysis of Laboratory-Active Belite Clinkers by Synchrotron Powder Diffraction, Journal of the American Ceramic Society, 90 (2007) 3205-3212. [132] X. Li, W. Xu, S. Wang, M. Tang, X. Shen, Effect of SO3 and MgO on Portland cement clinker: Formation of clinker phases and alite polymorphism, Construction and Building Materials, 58 (2014) 182-192. [133] K. Fukuda, I. Maki, K. Toyoda, S. Ito, Kinetics of the α-to-α′H Polymorphic Phase Transition of Ca2SiO4 Solid Solutions, Journal of the American Ceramic Society, 76 (1993) 1821-1824. [134] I. Jelenić, A. Bezjak, M. Bujan, Hydration of B2O3-stabilized α′-and β-modifications of dicalcium silicate, Cement and Concrete Research, 8 (1978) 173-180. [135] Y.-M. Kim, S.-H. Hong, Influence of Minor Ions on the Stability and Hydration Rates of β-Dicalcium Silicate, Journal of the American Ceramic Society, 87 (2004) 900-905. [136] R. Trettin, G. Oliew, C. Stadelmann, W. Wieker, Very early hydration of dicalcium silicate-polymorphs, Cement and Concrete Research, 21 (1991) 757-764. [137] K. Fukuda, H. Taguchi, Hydration of α′L- and β-dicalcium silicates with identical concentration of phosphorus oxide, Cement and Concrete Research, 29 (1999) 503-506. [138] A.J.M. Cuberos, Á.G. De la Torre, M.C. Martín-Sedeño, L. Moreno-Real, M. Merlini, L.M. Ordónez, M.A.G. Aranda, Phase development in conventional and active belite cement pastes by Rietveld analysis and chemical constraints, Cement and Concrete Research, 39 (2009) 833-842. [139] L. Nicoleau, A. Nonat, D. Perrey, The di- and tricalcium silicate dissolutions, Cement and Concrete Research, 47 (2013) 14-30. [140] D. Damidot, F. Bellmann, B. Möser, T. Sovoidnich, Calculation of the dissolution rate of tricalcium silicate in several electrolyte compositions, Cement Wapno Beton, 12/74 (2007) 57-67. [141] P. Suraneni, M. Palacios, R.J. Flatt, New insights into the hydration of slag in alkaline media using a micro-reactor approach, Cement and Concrete Research, 79 (2016) 209-216. [142] F. Bellmann, D. Damidot, B. Möser, J. Skibsted, Improved evidence for the existence of an intermediate phase during hydration of tricalcium silicate, Cement and Concrete Research, 40 (2010) 875-884. [143] V. Kocaba, Development and evaluation of methods to follow microstructural development of cementitious systems including slags, in: Laboratoire des matériaux de construction, EPFL, 2009, pp. 145. [144] M.J. Whittaker, The Impact of Slag Composition on the Microstructure of Composite Slag Cements Exposed to Sulfate Attack, in: School of Civil Engineering University of Leeds, 2015, pp. 116. [145] A.C.A. Muller, K.L. Scrivener, A.M. Gajewicz, P.J. McDonald, Densification of C–S–H Measured by 1H NMR Relaxometry, The Journal of Physical Chemistry C, 117 (2013) 403-412. [146] W.A. Gutteridge, J.A. Dalziel, Filler cement: The effect of the secondary component on the hydration of Portland cement: Part I. A fine non-hydraulic filler, Cement and Concrete Research, 20 (1990) 778-782. [147] R.J. Flatt, G.W. Scherer, J.W. Bullard, Why alite stops hydrating below 80% relative humidity, Cement and Concrete Research, 41 (2011) 987-992. [148] F.A. Steele, W.P. Davey, THE CRYSTAL STRUCTURE OF TRICALCIUM ALUMINATE, Journal of the American Chemical Society, 51 (1929) 2283-2293. [149] P. Mondal, J.W. Jeffery, The crystal structure of tricalcium aluminate, Ca3Al2O6, Acta Cryst, B31 (1975) 689-697. [150] L. Gobbo, L.l. Sant'Agostino, L. Garcez, C3A polymorphs related to industrial clinker alkalies content, Cement and Concrete Research, 34 (2004) 657-664. [151] S.P. Varma, C.D. Wall, A monoclinic tricalcium aluminate (C3A) phase in a commercial Portland cement clinker, Cement and Concrete Research, 11 (1981) 567-574. [152] R.M. Herath Banda, F.P. Glasser, Crystallization of the molten phase in portland cement clinker, Cement and Concrete Research, 8 (1978) 665-670. [153] E. Breval, C3A hydration, Cement and Concrete Research, 6 (1976) 129-137. [154] L. Black, C. Breen, J. Yarwood, C.-S. Deng, J. Phipps, G. Maitland, Hydration of tricalcium aluminate (C3A) in the presence and absence of gypsum—studied by Raman spectroscopy and X-ray diffraction, Journal of Material Chemistry, 16 (2006) 1263 - 1272. [155] H.J. Kuzel, H. Pöllmann, Hydration of C3A in the presence of Ca(OH)2, CaSO4·2H2O and CaCO3, Cement and Concrete Research, 21 (1991) 885-895. [156] P. Meredith, A. Donald, N. Meller, C. Hall, Tricalcium aluminate hydration: Microstructural observations by in-situ electron microscopy, Journal of materials science, 39 (2004) 997-1005. [157] T.D. Ciach, E.G. Swenson, Morphology and microstructure of hydrating portland cement and its constituents I. Changes in hydration of tricalcium aluminate alone and in the presence of triethanolamine or calcium lignosulphonate, Cement and Concrete Research, 1 (1971) 143-158. [158] D. Stephan, S. Wistuba, Crystal structure refinement and hydration behaviour of doped tricalcium aluminate, Cement and Concrete Research, 36 (2006) 2011-2020. [159] M. Collepardi, G. Baldini, M. Pauri, M. Corradi, Tricalcium aluminate hydration in the presence of lime, gypsum or sodium sulfate, Cement and Concrete Research, 8 (1978) 571-580. [160] P. Hewlett, Lea's chemistry of cement and concrete, Butterworth-Heinemann, 2003. [161] H. Taylor, Cement chemistry, (1997). [162] J. Pourchez, P. Grosseau, B. Ruot, Current understanding of cellulose ethers impact on the hydration of C3A and C3A-sulphate systems, Cement and Concrete Research, 39 (2009) 664-669. [163] H. Minard, S. Garrault, L. Regnaud, A. Nonat, Mechanisms and parameters controlling the tricalcium aluminate reactivity in the presence of gypsum, Cement and Concrete Research, 37 (2007) 1418-1426. [164] L. Amathieu, T.A. Bier, K. Scrivener, Mechanisms of set acceleration of Portland cement through CAC addition, in: International conference on calcium aluminate cements, 2001, pp. 303-317. [165] P.K. Mehta, Effect of lime on hydration of pastes containing gypsum and calcium aluminates or calcium sulfoaluminate, Journal of the American Ceramic Society, 56 (1973) 315-319. [166] A.P. Kirchheim, V. Fernandez-Altable, P.J.M. Monteiro, D.C.C. Dal Molin, Analysis of cubic and orthorhombic C3A hydration in presence of gypsum and lime, Journal of Materials Science, 44 (2009) 2038 - 2045. [167] D.A. Silva, P.J. Monteiro, Early formation of ettringite in tricalcium aluminate–calcium hydroxide–gypsum dispersions, Journal of the American Ceramic Society, 90 (2007) 614-617. [168] J. Skalny, M. Tadros, Retardation of tricalcium aluminate hydration by sulfates, Journal of the American Ceramic Society, 60 (1977) 174-175. [169] M. Merlini, G. Artioli, T. Cerulli, F. Cella, A. Bravo, Tricalcium aluminate hydration in additivated systems. A crystallographic study by SR-XRPD, Cement and Concrete Research, 38 (2008) 477-486. [170] R.F. Feldman, V.S. Ramachandran, The influence of CaSO4.2H2O upon the hydration character of 3CaO.Al2O3, Magazine of Concrete Research, 18 (1966) 185 –196. [171] P. Gupta, S. Chatterji, J. Jeffery, Cement Technology 4, in, I-4, 1973. [172] H.J. Kuzel, Initial hydration reactions and mechanisms of delayed ettringite formation in Portland cements, Cement and Concrete Composites, 18 (1996) 195-203. [173] T. Matschei, B. Lothenbach, F.P. Glasser, The role of calcium carbonate in cement hydration, Cement and Concrete Research, 37 (2007) 551-558. [174] T. Matschei, B. Lothenbach, F.P. Glasser, The AFm phase in Portland cement, Cement and Concrete Research, 37 (2007) 118-130. [175] J.J. Beaudoin, V.S. Ramachandran, A new perspective on the hydration characteristics of cement phases, Cement and Concrete Research, 22 (1992) 689-694. [176] A. Quennoz, K.L. Scrivener, Hydration of C3A–gypsum systems, Cement and Concrete Research, 42 (2012) 1032-1041. [177] K. De Weerdt, K.O. Kjellsen, E. Sellevold, H. Justnes, Synergy between fly ash and limestone powder in ternary cements, Cement and Concrete Composites, 33 (2011) 30-38. [178] M. Zajac, A. Rossberg, G. Le Saout, B. Lothenbach, Influence of limestone and anhydrite on the hydration of Portland cements, Cement and Concrete Composites, 46 (2014) 99-108. [179] J.J. Beaudoin, V. Ramachandran, A new perspective on the hydration characteristics of cement phases, Cement and Concrete research, 22 (1992) 689-694. [180] C. Plowman, J. Cabrera, Mechanism and kinetics of hydration of C3A and C4AF. Extracted from cement, Cement and Concrete Research, 14 (1984) 238-248. [181] D.E. Rogers, L.P. Aldridge, Hydrates of calcium ferrites and calcium aluminoferrites, Cement and Concrete Research, 7 (1977) 399-409. [182] B.Z. Dilnesa, B. Lothenbach, G. Renaudin, A. Wichser, D. Kulik, Synthesis and characterization of hydrogarnet Ca3(AlxFe1 − x)2(SiO4)y(OH)4(3 − y), Cement and Concrete Research, 59 (2014) 96-111. [183] B.Z. Dilnesa, E. Wieland, B. Lothenbach, R. Dähn, K.L. Scrivener, Fe-containing phases in hydrated cements, Cement and Concrete Research, 58 (2014) 45-55. [184] B.Z. Dilnesa, B. Lothenbach, G. Renaudin, A. Wichser, E. Wieland, Stability of monosulfate in the presence of iron, Journal of the American Ceramic Society, 95 (2012) 3305-3316. [185] B.Z. Dilnesa, B. Lothenbach, G. Le Saout, G. Renaudin, A. Mesbah, Y. Filinchuk, A. Wichser, E. Wieland, Iron in carbonate containing AFm phases, Cement and Concrete Research, 41 (2011) 311-323. [186] G. Renaudin, A. Mesbah, B. Zeleke Dilnesa, M. Francois, B. Lothenbach, Crystal chemistry of iron containing cementitious AFm layered hydrates, Current Inorganic Chemistry, 5 (2015) 184-193. [187] B. EN197-1, Cement: composition, specifications and conformity criteria for common cements, British Standards Institution, London, (2011). [188] M. Öner, A study of intergrinding and separate grinding of blast furnace slag cement, Cement and Concrete Research, 30 (2000) 473-480. [189] H.M. Jennings, Colloid model of C−S−H and implications to the problem of creep and shrinkage Materials and Structures, 37 (2004) 59-70. [190] X. Wu, D.M. Roy, C.A. Langton, Early stage hydration of slag-cement, Cement and Concrete Research, 13 (1983) 277-286. [191] C. Çetin, S.T. Erdoğan, M. Tokyay, Effect of particle size and slag content on the early hydration of interground blended cements, Cement and Concrete Composites, 67 (2016) 39-49. [192] G. Puerta-Falla, A. Kumar, L. Gomez-Zamorano, M. Bauchy, N. Neithalath, G. Sant, The influence of filler type and surface area on the hydration rates of calcium aluminate cement, Construction and Building Materials, 96 (2015) 657-665. [193] K.L. Scrivener, A. Nonat, Hydration of cementitious materials, present and future, Cement and Concrete Research, 41 (2011) 651-665. [194] J. Duchesne, M.A. Be´rube´, Effect of supplementary cementing materials on the composition of cement hydration products, Advanced Cement Based Materials, 2 (1995) 43-52. [195] I.G. Richardson, A.R. Brough, G.W. Groves, C.M. Dobson, The characterization of hardened alkali-activated blast-furnace slag pastes and the nature of the calcium silicate hydrate (C-S-H) phase, Cement and Concrete Research, 24 (1994) 813-829. [196] J.I. Escalante-Garcia, J.H. Sharp, The chemical composition and microstructure of hydration products in blended cements, Cement and Concrete Composites, 26 (2004) 967-976. [197] M. Öner, K. Erdoğdu, A. Günlü, Effect of components fineness on strength of blast furnace slag cement, Cement and Concrete Research, 33 (2003) 463-469. [198] S. Kumar, R. Kumar, A. Bandopadhyay, T.C. Alex, B. Ravi Kumar, S.K. Das, S.P. Mehrotra, Mechanical activation of granulated blast furnace slag and its effect on the properties and structure of portland slag cement, Cement and Concrete Composites, 30 (2008) 679-685. [199] M.B. Haha, B. Lothenbach, G. Le Saout, F. Winnefeld, Influence of slag chemistry on the hydration of alkali-activated blast-furnace slag — Part II: Effect of Al2O3, Cement and Concrete Research, 42 (2012) 74-83. [200] I. Ismail, S.A. Bernal, J.L. Provis, R. San Nicolas, S. Hamdan, J.S.J. van Deventer, Modification of phase evolution in alkali-activated blast furnace slag by the incorporation of fly ash, Cement and Concrete Composites, 45 (2014) 125-135. [201] A. Schöler, B. Lothenbach, F. Winnefeld, M. Zajac, Hydration of quaternary Portland cement blends containing blast-furnace slag, siliceous fly ash and limestone powder, Cement and Concrete Composites, 55 (2015) 374-382. [202] M.B. Haha, B. Lothenbach, G. Le Saout, F. Winnefeld, Influence of slag chemistry on the hydration of alkali-activated blast-furnace slag — Part I: Effect of MgO, Cement and Concrete Research, 41 (2011) 955-963. [203] R. Snellings, Solution-controlled dissolution of supplementary cementitious material glasses at pH 13: The effect of solution composition on glass dissolution rates, J Am Ceram Soc, 96 (2013) 2467–2475. [204] C. Shi, R.L. Day, Some factors affecting early hydration of alkali-slag cements, Cement and Concrete Research, 26 (1996) 439-447. [205] J.I. Escalante-García, A.F. Fuentes, A. Gorokhovsky, P.E. Fraire-Luna, G. Mendoza-Suarez, Hydration Products and Reactivity of Blast-Furnace Slag Activated by Various Alkalis, Journal of the American Ceramic Society, 86 (2003) 2148-2153. [206] S.A. Bernal, R. San Nicolas, R.J. Myers, R. Mejía de Gutiérrez, F. Puertas, J.S.J. van Deventer, J.L. Provis, MgO content of slag controls phase evolution and structural changes induced by accelerated carbonation in alkali-activated binders, Cement and Concrete Research, 57 (2014) 33-43. [207] I.G. Richardson, J.G. Cabrera, The nature of CSH in model slag-cements, Cement and Concrete Composites, 22 (2000) 259-266. [208] N. Mobasher, S.A. Bernal, J.L. Provis, Structural evolution of an alkali sulfate activated slag cement, Journal of Nuclear Materials, 468 (2016) 97-104. [209] A.M. Rashad, Influence of different additives on the properties of sodium sulfate activated slag, Construction and Building Materials, 79 (2015) 379-389. [210] I.G. Richardson, Tobermorite/jennite- and tobermorite/calcium hydroxide-based models for the structure of C-S-H: applicability to hardened pastes of tricalcium silicate, β-dicalcium silicate, Portland cement, and blends of Portland cement with blast-furnace slag, metakaolin, or silica fume, Cement and Concrete Research, 34 (2004) 1733-1777. [211] I.G. Richardson, G.W. Groves, The structure of the calcium silicate hydrate phases present in hardened pastes of white Portland cement/blast-furnace slag blends, Journal of material Science, 32 (1997) 4793-4802. [212] E. Tajuelo Rodriguez, I.G. Richardson, L. Black, E. Boehm-Courjault, A. Nonat, J. Skibsted, Composition, silicate anion structure and morphology of calcium silicate hydrates (C-S-H) synthesised by silica-lime reaction and by controlled hydration of tricalcium silicate (C3S), Advances in Applied Ceramics, 114 (2015) 362-371. [213] M. Vandamme, F.-J. Ulm, P. Fonollosa, Nanogranular packing of C–S–H at substochiometric conditions, Cement and Concrete Research, 40 (2010) 14-26. [214] K. J. Krakowiak, W. Wilson, S. James, S. Musso, F.-J. Ulm, Inference of the phase-to-mechanical property link via coupled X-ray spectrometry and indentation analysis: Application to cement-based materials, Cement and Concrete Research, 67 (2015) 271-285. [215] S.P. Pandey, R.L. Sharma, The influence of mineral additives on the strength and porosity of OPC mortar, Cement and Concrete Research, 30 (2000) 19-23. [216] D.P. Bentz, Modeling the influence of limestone filler on cement hydration using CEMHYD3D, Cement and Concrete Composites, 28 (2006) 124-129. [217] I. Soroka, N. Stern, Calcareous fillers and the compressive strength of portland cement, Cement and Concrete Research, 6 (1976) 367-376. [218] I. Soroka, N. Setter, The effect of fillers on strength of cement mortars, Cement and Concrete Research, 7 (1977) 449-456. [219] V. Bonavetti, H. Donza, G. Menéndez, O. Cabrera, E.F. Irassar, Limestone filler cement in low w/c concrete: A rational use of energy, Cement and Concrete Research, 33 (2003) 865-871. [220] E.F. Irassar, D. Violini, V.F. Rahhal, C. Milanesi, M.A. Trezza, V.L. Bonavetti, Influence of limestone content, gypsum content and fineness on early age properties of Portland limestone cement produced by inter-grinding, Cement and Concrete Composites, 33 (2011) 192-200. [221] A.-M. Poppe, G. De Schutter, Cement hydration in the presence of high filler contents, Cement and Concrete Research, 35 (2005) 2290-2299. [222] M. Nehdi, S. Mindess, P.-C. Aïtcin, Optimization of high strength limestone filler cement mortars, Cement and Concrete Research, 26 (1996) 883-893. [223] T. Matschei, B. Lothenbach, F.P. Glasser, Thermodynamic properties of Portland cement hydrates in the system CaO–Al 2 O 3–SiO 2–CaSO 4–CaCO 3–H 2 O, Cement and Concrete Research, 37 (2007) 1379-1410. [224] G. Ye, X. Liu, G. De Schutter, A.M. Poppe, L. Taerwe, Influence of limestone powder used as filler in SCC on hydration and microstructure of cement pastes, Cement and Concrete Composites, 29 (2007) 94-102. [225] P. Mounanga, M.I.A. Khokhar, R. Hachem, A. Loukili, Improvement of the early-age reactivity of fly ash and blast furnace slag cementitious systems using limestone filler, Materials and Structures, 44 (2011) 437-453. [226] Y. Zhang, G. Ye, Effect of Limestone Powder on Microstructure of Ternary Cementitious System., Sustainable Construction Materials (2012) 225-234. [227] W.A. Klemm, L.D. Adams, An investigation of the formation of carboaluminates in: P. Klieger, R.D. Hooton (Eds.) Carbonate Additions to Cement, ASTM STP 1064, American Society for Testing and Materials, Philadelphia, 1990, pp. 60-72. [228] L. Basheer, J. Kropp, D.J. Cleland, Assessment of the durability of concrete from its permeation properties: a review, Construction and Building Materials, 15 (2001) 93-103. [229] P.H.R. Borges, J.O. Costa, N.B. Milestone, C.J. Lynsdale, R.E. Streatfield, Carbonation of CH and C–S–H in composite cement pastes containing high amounts of BFS, Cement and Concrete Research, 40 (2010) 284-292. [230] J.J. Chen, J.J. Thomas, H.M. Jennings, Decalcification shrinkage of cement paste, Cement and Concrete Research, 36 (2006) 801-809. [231] J. Kim, W.J. McCarter, B. Suryanto, S. Nanukuttan, P.A.M. Basheer, T.M. Chrisp, Chloride ingress into marine exposed concrete: A comparison of empirical- and physically- based models, Cement and Concrete Composites, 72 (2016) 133-145. [232] U. Balters, U. Ludwig, Influence of cement type on resistance against freezing and thawing, with or without deicing chemicals, of cement mortar, Frost Resistance of Concrete, 34 (2004) 119. [233] A. Marciniak, W. Grymin, T. Margiewicz, M. Koniorczyk, Influence of freezing-induced damage on the carbonation rate of concrete, European Journal of Environmental and Civil Engineering, (2016) 1-16. [234] J. Stark, A. Eckart, H.M. Ludwig, Influence of C3A content on frost and scaling resistance, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop on Resistance of Concrete to Freezing and Thawing With or Without De-icing Chemicals, E & FN SPON, University of Essen, 1997, pp. 100-109. [235] H. Toutanji, N. Delatte, S. Aggoun, R. Duval, A. Danson, Effect of supplementary cementitious materials on the compressive strength and durability of short-term cured concrete, Cement and Concrete Research, 34 (2004) 311-319. [236] G.J. Osborne, Durability of Portland blast-furnace slag cement concrete, Cement and Concrete Composites, 21 (1999) 11-21. [237] L.J. Parrott, Some effects of cement and curing upon carbonation and reinforcement corrosion in concrete, Materials and Structures, 29 (1996) 164-173 [238] O. Wowra, Effects of carbonation to microstructure and pore solution, in: N.J. Setzer, R. Auberg, I.J. Keck (Eds.) International RILEM Workshop on Frost Resistance of Concrete, 2002, pp. 61 - 68. [239] T. Grounds, H. Midgley, D. Novell, Carbonation of ettringite by atmospheric carbon dioxide, Thermochimica Acta, 135 (1988) 347-352. [240] E. Dubina, L. Korat, L. Black, J. Strupi-Šuput, J. Plank, Influence of water vapour and carbon dioxide on free lime during storage at 80 C, studied by Raman spectroscopy, Spectrochimica Acta Part A: Molecular and Biomolecular Spectroscopy, 111 (2013) 299-303. [241] L. Black, K. Garbev, I. Gee, Surface carbonation of synthetic CSH samples: A comparison between fresh and aged CSH using X-ray photoelectron spectroscopy, Cement and Concrete Research, 38 (2008) 745-750. [242] Z. Šauman, Effect of CO2 on porous concrete, Cement and Concrete Research, 2 (1972) 541-549. [243] E. Gruyaert, P. Van den Heede, N. De Belie, Carbonation of slag concrete: Effect of the cement replacement level and curing on the carbonation coefficient – Effect of carbonation on the pore structure, Cement and Concrete Composites, 35 (2013) 39-48. [244] E.T. Stepkowska, J.L. Pérez-Rodríguez, M.J. Sayagués, J.M. Martínez-Blanes, Calcite, vaterite and aragonite forming on cement hydration from liquid and gaseous phase, Journal of Thermal Analysis and Calorimetry 73 (2003) 247 - 269. [245] D. Russell, P.A.M. Basheer, G.I.B. Rankin, A.E. Long, Effect of relative humidity and air permeability on prediction of the rate of carbonation of concrete, Proceedings of the ICE - Structures and Buildings, 146 (2001) 319 - 326. [246] D.W.S. Ho, Q.Y. Cui, D.J. Ritchie, The influence of humidity and curing time on the quality of concrete, Cement and Concrete Research, 19 (1989) 457-464. [247] Z. Šauman, Carbonization of porous concrete and its main binding components, Cement and Concrete Research, 1 (1971) 645-662. [248] Z. Hu, M. Shao, Q. Cai, S. Ding, C. Zhong, X. Wei, Y. Deng, Synthesis of needle-like aragonite from limestone in the presence of magnesium chloride, Journal of Materials Processing Technology, 209 (2009) 1607-1611. [249] P. Pipilikaki, M. Beazi-Katsioti, The assessment of porosity and pore size distribution of limestone Portland cement pastes, Construction and Building Materials, 23 (2009) 1966-1970. [250] O. Çopuroğlu, A.L.A. Fraaij, J.M.J.M. Bijen, Effect of sodium monofluorophosphate treatment on microstructure and frost salt scaling durability of slag cement paste, Cement and Concrete Research, 36 (2006) 1475-1482. [251] B. Johannesson, P. Utgenannt, Microstructural changes caused by carbonation of cement mortar, Cement and Concrete Research, 31 (2001) 925-931. [252] G. Fagerlund, Internal frost attack - State of the art, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop, Essen, 1997, pp. 321 - 338. [253] H.-J. Chen, S.-S. Huang, C.-W. Tang, M.A. Malek, L.-W. Ean, Effect of curing environments on strength, porosity and chloride ingress resistance of blast furnace slag cement concretes: A construction site study, Construction and Building Materials, 35 (2012) 1063-1070. [254] V.T. Ngala, C.L. Page, EFFECTS OF CARBONATION ON PORE STRUCTURE AND DIFFUSIONAL PROPERTIES OF HYDRATED CEMENT PASTES, Cement and Concrete Research, 27 (1997) 995-1007. [255] M. Pigeon, M. Setzer, ACTION OF FROST AND DEICING CHEMICALS-BASIC PHENOMENA AND TESTING, RILEM PROCEEDINGS 30 FREEZE-THAW DURABILITY OF CONCRETE, (1997). [256] J.J. Beaudoin, C. MacInnis, The mechanism of frost damage in hardened cement paste, Cement and Concrete Research, 4 (1974) 139-147. [257] M. Setzer, Action of frost and deicing chemicals: basic phenomena and testing, Freeze Thaw Durability of Concrete, (1976) 3-21. [258] O. Coussy, P.J.M. Monteiro, Poroelastic model for concrete exposed to freezing temperatures, Cement and Concrete Research, 38 (2008) 40-48. [259] O. Coussy, P. Monteiro, Unsaturated poroelasticity of freezing water-infiltrated materials with air voids, in: Poromechanics III-Biot Centennial (1905-2005): Proceedings of the 3rd Biot Conference on Poromechanics, 24-27 May 2005, Norman, Oklahoma, USA, CRC Press, 2005, pp. 457. [260] G.J. Verbeck, P. Klieger, Studies of'salt'scaling of concrete, Highway Research Board Bulletin, (1957). [261] O. Çopuroğlu, E. Schlangen, Modeling of frost salt scaling, Cement and Concrete Research, 38 (2008) 27-39. [262] V. Penttala, Surface and internal deterioration of concrete due to saline and non-saline freeze–thaw loads, Cement and Concrete Research, 36 (2006) 921-928. [263] J.S. Walder, B. Hallet, The physical basis of frost weathering: Toward a more fundamental and unified perspective, Artic and Alpine Research, 18 (1986) 27-32. [264] D.R. Uhlmann, B. Chalmers, K.A. Jackson, Interaction Between Particles and a Solid‐Liquid Interface, Journal of Applied Physics, 35 (1964) 2986-2993. [265] D.J. Janssen, The influence of material parameters on freeze-thaw resistance with and without deicing salt, in: M.J. Setzer, R. Auberg (Eds.) Proceedings of the Internal RILEM Workshop on Resistance of Concrete to Freezing and Thawing with or without De-icing Chemicals E&FN SPON, University of Essen, 1997, pp. 3-10. [266] A. Bilodeau, V.M. Malhotra, Deicing salt scaling resistance of concrete incorporating supplementary cementious materials: CANMET Research, in: J. Marchand, M. Pigeon, M. Setzer (Eds.) RILEM PROCEEDINGS 30 FREEZE-THAW DURABILITY OF CONCRETE, E and F Spon Limited, Quebec, Canada, 1997, pp. 121-156. [267] T.F. Rønning, Freeze-Thaw Resistance of Concrete: Effect of: Curing Conditions, Moisture Exchange and Materials, (2001). [268] W. Sun, Y.M. Zhang, H.D. Yan, R. Mu, Damage and damage resistance of high strength concrete under the action of load and freeze-thaw cycles, Cement and Concrete Research, 29 (1999) 1519-1523. [269] Z. Giergiczny, M.A. Glinicki, M. Sokołowski, M. Zielinski, Air void system and frost-salt scaling of concrete containing slag-blended cement, Construction and Building Materials, 23 (2009) 2451-2456. [270] C. Girodet, M. Chabannet, J. Bosc, J. Pera, Influence of the type of cement on the freeze-thaw resistance of the mortar phase of concrete, Frost Resistance of Concrete, 34 (2004) 34. [271] P. Taylor, Effect of Clinker Chemistry on Salt Scaling Resistance of Concrete, Transportation Research Record: Journal of the Transportation Research Board, 2113 (2009) 108-113. [272] H.F.W. Taylor, C. Famy, K.L. Scrivener, Delayed ettringite formation, Cement and Concrete Research, 31 (2001) 683-693. [273] A. Müller, C. Fuhr, D. Knöfel, Frost resistance of cement mortars with different lime contents, Cement and concrete research, 25 (1995) 809-818. [274] R. Bleszynski, R.D. Hooton, M.D. Thomas, C.A. Rogers, Durability of ternary blend concrete with silica fume and blast-furnace slag: laboratory and outdoor exposure site studies, ACI Materials Journal, 99 (2002) 499-508. [275] S.E. Chidiac, D.K. Panesar, Evolution of mechanical properties of concrete containing ground granulated blast furnace slag and effects on the scaling resistance test at 28days, Cement and Concrete Composites 30 (2008) 63-71 [276] M.S. Meddah, M.C. Lmbachiya, R.K. Dhir, Potential use of binary and composite limestone cements in concrete production, Construction and Building Materials, 58 (2014) 193-205. [277] B. Li, J. Wang, M. Zhou, Effect of limestone fines content in manufactured sand on durability of low- and high-strength concretes, Construction and Building Materials, 23 (2009) 2846-2850. [278] B. Espion, B. Lebon, C. Pierre, O. Germain, A. Hellebois, Characterisation of new ternary cements with reduced clinker content, in: Proceedings of the First International Conference on Concrete Sustainability, Japan Concrete Institute, 2013, pp. 145-152. [279] I.K. Battaglia, J.F. Munoz, S.M. Cramer, Proposed behavioral model for deicer scaling resistance of slag cement concrete, J Mater CivEng, 22 (2011) 361-368. [280] O. Çopuro, L. Fraaij, J. Bijen, Effect of curing conditions on freeze-thaw de-icing salt resistance of blast furnace slag cement mortars, WIT Transactions on The Built Environment, 76 (2004). [281] R.M. Geiker, Studies of Portland Cement Hydration: Measurements of Chemical Shrinkage and a Systematic Evaluaiton of Hydration Curves by Means of Dispersion Model, in: Technical University of Denmark, Technical University of Denmark, Technical University of Denmark, 1983. [282] J. Hjorth, J. Skibsted, H.J. Jakobsen, 29Si MAS NMR studies of portland cement components and effects of microsilica on the hydration reaction, Cement and Concrete Research, 18 (1988) 789-798. [283] A. Bentur, Effect of Gypsum on the Hydration and Strength of C3S Pastes, American Ceramic Society, 59 (1976) 210-213. [284] D. Ménétrier, I. Jawed, J. Skalny, Effect of gypsum on C3S hydration, Cement and Concrete Research, 10 (1980) 697-701. [285] I. Pane, W. Hansen, Investigation of blended cement hydration by isothermal calorimetry and thermal analysis, Cement and Concrete Research, 35 (2005) 1155-1164. [286] I. Wadsö, L. Wadsö, Systematic errors in isothermal micro-and nanocalorimetry, Journal of thermal analysis and calorimetry, 82 (2005) 553-558. [287] L. Wadsö, Operational issues in isothermal calorimetry, Cement and Concrete Research, 40 (2010) 1129-1137. [288] S.T. Bergold, F. Goetz-Neunhoeffer, J. Neubauer, Influence of the reactivity of the amorphous part of mechanically activated alite on its hydration kinetics, Cement and Concrete Research, 88 (2016) 73-81. [289] J.L. Poole, K.A. Riding, K.J. Folliard, M.C. Juenger, A.K. Schindler, Methods for calculating activation energy for Portland cement, ACI Materials Journal, 104 (2007) 86. [290] A. C1608-12, Standard Test Method for Chemical Shrinkage of Hydraulic Cement Paste, in, ASTM International, West Conshohocken, PA, 2012. [291] N. Setter, D.M. Roy, Mechanical features of chemical shrinkage of cement paste, Cement and Concrete Research, 8 (1978) 623-634. [292] T.C. Powers, T.L. Brownyard, Studies of the physical properties of hardened Portland cement paste, in: Journal Proceedings, 1946, pp. 101-132. [293] H.J.H. Brouwers, The work of Powers and Brownyard revisited: Part 1, Cement and Concrete Research, 34 (2004) 1697-1716. [294] M. Geiker, T. Knudsen, Chemical shrinkage of portland cement pastes, Cement and Concrete Research, 12 (1982) 603-610. [295] S. Boivin, P. Acker, S. Rigaud, B. Clavaud, Experimental assessment of chemical shrinkage of hydrating cement pastes, in: Autogenous shrinkage of concrete Spon Press, Proceedings of the International Workshop organized by the JCI (Japan Concrete Institute), 1999, pp. 81-92. [296] P. Lura, F. Winnefeld, S. Klemm, Simultaneous measurements of heat of hydration and chemical shrinkage on hardening cement pastes, Journal of Thermal Analysis and Calorimetry, 101 (2010) 925-932. [297] F. Lin, C. Meyer, Hydration kinetics modeling of Portland cement considering the effects of curing temperature and applied pressure, Cement and Concrete Research, 39 (2009) 255-265. [298] L.J. Parrott, M. Geiker, W.A. Gutteridge, D. Killoh, Monitoring Portland cement hydration: Comparison of methods, Cement and Concrete Research, 20 (1990) 919-926. [299] H.M. Dyson, I.G. Richardson, A.R. Brough, A Combined 29Si MAS NMR and Selective Dissolution Technique for the Quantitative Evaluation of Hydrated Blast Furnace Slag Cement Blends, J Am Ceram Soc, 90 (2007) 598-602. [300] L. McCusker, R. Von Dreele, D. Cox, D. Louer, P. Scardi, Rietveld refinement guidelines, Journal of Applied Crystallography, 32 (1999) 36-50. [301] G. Le Saoût, V. Kocaba, K. Scrivener, Application of the Rietveld method to the analysis of anhydrous cement, Cement and concrete research, 41 (2011) 133-148. [302] L. Mitchell, P. Whitfield, J. Beaudoin, The effects of particle statistics on quantitative Rietveld analysis of cement, in: 12th International congress on the Chemistry of Cement, Montreal, 2007, pp. 1-12. [303] R. Snellings, A. Bazzoni, K. Scrivener, The existence of amorphous phase in Portland cements: Physical factors affecting Rietveld quantitative phase analysis, Cement and Concrete Research, 59 (2014) 139-146. [304] W. Dollase, Correction of intensities for preferred orientation in powder diffractometry: application of the March model, Journal of Applied Crystallography, 19 (1986) 267-272. [305] N.C. Popa, Microstructural properties: Texture and macrostress effects, Chapter, 12 (2008) 332-375. [306] R. Von Dreele, Quantitative texture analysis by Rietveld refinement, Journal of Applied Crystallography, 30 (1997) 517-525. [307] D.L. Bish, S. Howard, Quantitative phase analysis using the Rietveld method, Journal of Applied Crystallography, 21 (1988) 86-91. [308] H. Rietveld, A profile refinement method for nuclear and magnetic structures, Journal of applied Crystallography, 2 (1969) 65-71. [309] K.L. Scrivener, T. Füllmann, E. Gallucci, G. Walenta, E. Bermejo, Quantitative study of Portland cement hydration by X-ray diffraction/Rietveld analysis and independent methods, Cement and Concrete Research, 34 (2004) 1541-1547. [310] D. Jansen, C. Stabler, F. Goetz-Neunhoeffer, S. Dittrich, J. Neubauer, Does Ordinary Portland Cement contain amorphous phase? A quantitative study using an external standard method, Powder Diffraction, 26 (2011) 31-38. [311] F.H. Chung, Quantitative interpretation of X-ray diffraction patterns of mixtures. I. Matrix-flushing method for quantitative multicomponent analysis, Journal of Applied Crystallography, 7 (1974) 519-525. [312] F.H. Chung, Quantitative interpretation of X-ray diffraction patterns of mixtures. III. Simultaneous determination of a set of reference intensities, Journal of Applied Crystallography, 8 (1975) 17-19. [313] D. Jansen, F. Goetz-Neunhoeffer, C. Stabler, J. Neubauer, A remastered external standard method applied to the quantification of early OPC hydration, Cement and Concrete Research, 41 (2011) 602-608. [314] P.M. Suherman, A. van Riessen, B. O’Connor, D. Li, D. Bolton, H. Fairhurst, Determination of amorphous phase levels in Portland cement clinker, Powder Diffraction, 17 (2002) 178-185. [315] G. Le Saout, K. Scrivener, Early Hydration of Portland Cement with Corundum Addition, in: 16 Internationale Baustofftagung (ibausil), Weimar, Germany, 2006, pp. 409-416. [316] A. De La Torre, S. Bruque, M. Aranda, Rietveld quantitative amorphous content analysis, Journal of Applied Crystallography, 34 (2001) 196-202. [317] I.C. Madsen, N.V. Scarlett, A. Kern, Description and survey of methodologies for the determination of amorphous content via X-ray powder diffraction, Zeitschrift für Kristallographie Crystalline Materials, 226 (2011) 944-955. [318] B.H. O'Connor, M.D. Raven, Application of the Rietveld refinement procedure in assaying powdered mixtures, Powder Diffraction, 3 (1988) 2-6. [319] C. Hesse, F. Goetz-Neunhoeffer, J. Neubauer, M. Braeu, P. Gaeberlein, Quantitative in situ X-ray diffraction analysis of early hydration of Portland cement at defined temperatures, Powder Diffraction, 24 (2009) 112-115. [320] S.T. Bergold, F. Goetz-Neunhoeffer, J. Neubauer, Quantitative analysis of C–S–H in hydrating alite pastes by in-situ XRD, Cement and Concrete Research, 53 (2013) 119-126. [321] N.C. Collier, J.H. Sharp, N.B. Milestone, J. Hill, I.H. Godfrey, The influence of water removal techniques on the composition and microstructure of hardened cement pastes, Cement and Concrete Research, 38 (2008) 737-744. [322] J. Zhang, G.W. Scherer, Comparison of methods for arresting hydration of cement, Cement and Concrete Research, 41 (2011) 1024-1036. [323] K.L. Scrivener, H. Patel, P. Pratt, L. Parrott, Analysis of phases in cement paste using backscattered electron images, methanol adsorption and thermogravimetric analysis, in: Mater Res Soc Symp Proc, Cambridge Univ Press, 1987, pp. 67-76. [324] P.J. Goodhew, J. Humphreys, R. Beanland, Electron microscopy and analysis, CRC Press, 2000. [325] H.S. Wong, M.K. Head, N.R. Buenfeld, Pore segmentation of cement-based materials from backscattered electron images, Cement and Concrete Research, 36 (2006) 1083-1090. [326] X. Feng, E.J. Garboczi, D.P. Bentz, P.E. Stutzman, T.O. Mason, Estimation of the degree of hydration of blended cement pastes by a scanning electron microscope point-counting procedure, Cement and Concrete Research, 34 (2004) 1787-1793. [327] T.C. Powers, Structure and physical properties of hardened Portland cement paste, Journal of the American Ceramic Society, 41 (1958) 1-6. [328] A.B. Abell, K.L. Willis, D.A. Lange, Mercury Intrusion Porosimetry and Image Analysis of Cement-Based Materials, Journal of Colloid and Interface Science, 211 (1999) 39-44. [329] S. Diamond, Mercury porosimetry: An inappropriate method for the measurement of pore size distributions in cement-based materials, Cement and Concrete Research, 30 (2000) 1517-1525. [330] P.J. McDonald, V. Rodin, A. Valori, Characterisation of intra- and inter-C–S–H gel pore water in white cement based on an analysis of NMR signal amplitudes as a function of water content, Cement and Concrete Research, 40 (2010) 1656-1663. [331] H. Elaqra, N. Godin, G. Peix, M. R'Mili, G. Fantozzi, Damage evolution analysis in mortar, during compressive loading using acoustic emission and X-ray tomography: Effects of the sand/cement ratio, Cement and Concrete Research, 37 (2007) 703-713. [332] E.W. Washburn, Note on a method of determining the distribution of pore sizes in a porous material, Proceedings of the National Academy of Sciences, 7 (1921) 115-116. [333] C. Gallé, Effect of drying on cement-based materials pore structure as identified by mercury intrusion porosimetry: A comparative study between oven-, vacuum-, and freeze-drying, Cement and Concrete Research, 31 (2001) 1467-1477. [334] L. Konecny, S. Naqvi, The effect of different drying techniques on the pore size distribution of blended cement mortars, Cement and concrete research, 23 (1993) 1223-1228. [335] H. Ma, Mercury intrusion porosimetry in concrete technology: tips in measurement, pore structure parameter acquisition and application, Journal of porous materials, 21 (2014) 207-215. [336] N. Hearn, R.D. Hooton, Sample mass and dimension effects on mercury intrusion porosimetry results, Cement and Concrete Research, 22 (1992) 970-980. [337] L. Tang, P.-E. Petersson, Slab test-freeze/Thaw resistance of concrete—Internal deterioration, Materials and Structures, 34 (2001) 526-531. [338] G.W. Scherer, Freezing gels, Journal of Non-Crystalline Solids, 155 (1993) 1-25. [339] B. Lothenbach, P. Durdzinski, K. De Weerdt, Chapter 5: Thermogravimetric Analysis, a practical guide to microstructural analysis of cementitious materials, Edt Karen Scrivener, Ruben Snellings, and Barbara Lothenbach, to be published byTaylor & Francis Group, (2016). [340] PDCEN/TR15177, Testing the freeze-thaw resistance of concrete-Internal structural damage, in, 2006. [341] E. Knapen, O. Cizer, K. Van Balen, D. Van Gemert, Effect of free water removal from early-age hydrated cement pastes on thermal analysis, Construction and Building Materials, 23 (2009) 3431-3438. [342] M. Whittaker, L. Black, Relationship between, early stage microstructure and long term durability of slag-containing cements, in: M. Russell (Ed.) 32nd Cement and Concrete Science Conference, Queens University Belfast, 2012, pp. 161-165. [343] L. Zhang, F. Glasser, Critical examination of drying damage to cement pastes, Advances in cement research, 12 (2000) 79-88. [344] R.L. Day, B.K. Marsh, Measurement of porosity in blended cement pastes, Cement and Concrete Research, 18 (1988) 63-73. [345] R.W. Cheary, A.A. Coelho, J.P. Cline, Fundamental parameters line profile fitting in laboratory diffractometers, J Res Natl Inst Stand Technol, 109 (2004) 1-25. [346] H. Morikawa, I. Minato, T. Tomita, S. Iwai, Anhydrite: a refinement, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 31 (1975) 2164-2165. [347] K. Ojima, Y. Nishihata, A. Sawada, Structure of potassium sulfate at temperatures from 296 K down to 15 K, Acta Crystallographica Section B: Structural Science, 51 (1995) 287-293. [348] H. Schmidt, I. Paschke, D. Freyer, W. Voigt, Water channel structure of bassanite at high air humidity: crystal structure of CaSO4· 0.625 H2O, Acta Crystallographica Section B: Structural Science, 67 (2011) 467-475. [349] W. Mumme, R. Hill, G. Bushnell-Wye, E. Segnit, Rietveld crystal structure refinements, crystal chemistry and calculated powder diffraction data for the polymorphs of dicalcium silicate and related phases, Neues Jahrbuch fur Mineralogie Abhandlungen, 169 (1995) 35-68. [350] A. Colville, S. Geller, The crystal structure of brownmillerite, Ca2FeAlO5, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 27 (1971) 2311-2315. [351] P. Mondal, J. Jeffery, The crystal structure of tricalcium aluminate, Ca3Al2O6, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 31 (1975) 689-697. [352] Y. Takeuchi, F. Nishi, Crystal-chemical characterization of the 3CaO· Al2O3—Na2O solid-solution series, Zeitschrift für Kristallographie-Crystalline Materials, 152 (1980) 259-308. [353] E. Maslen, V. Streltsov, N. Streltsova, N. Ishizawa, Electron density and optical anisotropy in rhombohedral carbonates. III. Synchrotron X-ray studies of CaCO3, MgCO3 and MnCO3, Acta Crystallographica Section B: Structural Science, 51 (1995) 929-939. [354] T. Pilati, F. Demartin, C. Gramaccioli, Lattice-dynamical estimation of atomic displacement parameters in carbonates: calcite and aragonite CaCO3, dolomite CaMg (CO3) 2 and magnesite MgCO3, Acta Crystallographica Section B: Structural Science, 54 (1998) 515-523. [355] G. Renaudin, R. Segni, D. Mentel, J.-M. Nedelec, F. Leroux, C. Taviot-Gueho, A Raman Study of the Sulfated Cement Hydrates: Ettringite and Monosulfoaluminate, Journal of Advanced Concrete Technology, 5 (2007) 299-312. [356] Á.G. De La Torre, S. Bruque, J. Campo, M.A. Aranda, The superstructure of C 3 S from synchrotron and neutron powder diffraction and its role in quantitative phase analyses, Cement and Concrete Research, 32 (2002) 1347-1356. [357] T. Runčevski, R.E. Dinnebier, O.V. Magdysyuk, H. Pöllmann, Crystal structures of calcium hemicarboaluminate and carbonated calcium hemicarboaluminate from synchrotron powder diffraction data, Acta Crystallographica Section B: Structural Science, 68 (2012) 493-500. [358] M. Bellotto, B. Rebours, O. Clause, J. Lynch, D. Bazin, E. Elkaïm, A reexamination of hydrotalcite crystal chemistry, The Journal of Physical Chemistry, 100 (1996) 8527-8534. [359] D. Taylor, Thermal expansion data. I: Binary oxides with the sodium chloride and wurtzite structures, MO, Transactions and journal of the British Ceramic Society, 83 (1984) 5-9. [360] D. Henderson, H. Gutowsky, A nuclear magnetic resonance determination of the hydrogen positions in Ca (OH) 2, in, DTIC Document, 1962. [361] Y. Le Page, G. Donnay, Refinement of the crystal structure of low-quartz, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 32 (1976) 2456-2459. [362] D.C. Creagh, J.H. Hubbell, X-ray absorption (or attenuation) coefficients, International Tables for Crystallography, C (2006) 220-229. [363] V.S. Ramachandran, R.M. Paroli, J.J. Beaudoin, A.H. Delgado, Handbook of Thermal Analysis of Construction Materials, in, NOYES Publications, 2002, pp. 72-136. [364] R.S. Barneyback Jr, S. Diamond, Expression and analysis of pore fluids from hardened cement pastes and mortars, Cement and Concrete Research, 11 (1981) 279-285. [365] P.S. Whitfield, L.D. Mitchell, Quantitative Rietveld analysis of the amorphous content in cements and clinkers, Journal of Materials Science, 38 (2003) 4415-4421. [366] P. Scardi, Microstructural properties: lattice defects and domain size effects, Powder Diffraction Theory and Practice, (2008) 376-413. [367] Q. Zhou, F.P. Glasser, Thermal stability and decomposition mechanisms of ettringite at <120°C, Cement and Concrete Research, 31 (2001) 1333-1339. [368] J.H. Hubbell, Review and history of photon cross section calculationsWork supported by the National Institute of Standards and Technology, Physics in medicine and biology, 51 (2006) R245. [369] R. Snellings, —X-ray powder diffraction applied to cement, A Practical Guide to Microstructural Analysis of Cementitious Materials, (2016) 107. [370] A. Arora, G. Sant, N. Neithalath, Ternary blends containing slag and interground/blended limestone: Hydration, strength, and pore structure, Construction and Building Materials, 102, Part 1 (2016) 113-124. [371] I. Jawed, J. Skalny, Alkalies in cement: A review, Cement and Concrete Research, 8 (1978) 37-51. [372] L. Opoczky, Grinding technical questions of producing composite cements, Int J Miner Process, 44-45 (1996) 395-404. [373] A. Kumar, G. Sant, C. Patapy, C. Gianocca, K.L. Scrivener, The influence of sodium and potassium hydroxide on alite hydration: Experiments and simulations, Cement and Concrete Research, 42 (2012) 1513-1523. [374] T. Vuk, V. Tinta, R. Gabrovšek, V. Kaučič, The effects of limestone addition, clinker type and fineness on properties of Portland cement, Cement and Concrete Research, 31 (2001) 135-139. [375] K. Vance, M. Aguayo, T. Oey, G. Sant, N. Neithalath, Hydration and strength development in ternary portland cement blends containing limestone and fly ash or metakaolin, Cement and Concrete Composites, 39 (2013) 93-103. [376] A. Gruskovnjak, B. Lothenbach, F. Winnefeld, B. Münch, R. Figi, S.-C. Ko, M. Adler, U. Mäder, Quantification of hydration phases in supersulfated cements: review and new approaches, Adv Cem Res, 23 (2011) 265-275. [377] P.Z. Wang, R. Trettin, V. Rudert, Effect of fineness and particle size distribution of granulated blast-furnace slag on the hydraulic reactivity in cement systems, Advances in Cement Research, 17 (2005) 161-166. [378] J. J. Biernacki, J. M. Richardson, P. E. Stutzman, D.P. Bentz, Kinetics of Slag Hydration in the Presence of Calcium Hydroxide, J Am Ceram Soc, 85 (2002) 2261–2267. [379] S.C. Pal, A. Mukherjee, S.R. Pathak, Investigation of hydraulic activity of ground granulated blast furnace slag in concrete, Cement and Concrete Research, 33 (2003) 1481-1486. [380] H. Zhang, Z. Lin, D. Tong, Influence of the type of calcium sulfate on the strength and hydration of portland cement under an initial steam-curing condition, Cement and concrete research, 26 (1996) 1505-1511. [381] J. Cheung, A. Jeknavorian, L. Roberts, D. Silva, Impact of admixtures on the hydration kinetics of Portland cement, Cement and Concrete Research, 41 (2011) 1289-1309. [382] D. Rothstein, J.J. Thomas, B.J. Christensen, H.M. Jennings, Solubility behavior of Ca-, S-, Al-, and Si-bearing solid phases in Portland cement pore solutions as a function of hydration time, Cement and Concrete Research, 32 (2002) 1663-1671. [383] P. Monteiro, P.K. Mehta, Interaction between carbonate rock and cement paste, Cement and Concrete Research, 16 (1986) 127-134. [384] M.T. Palou, J. Majling, Effects of sulphate, calcium and aluminum ions upon the hydration of sulphoaluminate belite cement, Journal of thermal analysis, 46 (1996) 549-556. [385] D. Bentz, G. Sant, J. Weiss, Early-Age Properties of Cement-Based Materials. I: Influence of Cement Fineness, Journal of Materials in Civil Engineering 20 (2008) 502–508. [386] M. Collepardi, G. Baldini, M. Pauri, M. Corradi, The effect of pozzolanas on the tricalcium aluminate hydration, Cement and Concrete Research, 8 (1978) 741-751. [387] J. Péra, S. Husson, B. Guilhot, Influence of finely ground limestone on cement hydration, Cement and Concrete Composites, 21 (1999) 99-105. [388] T. Oey, A. Kumar, J.W. Bullard, N. Neithalath, G. Sant, The Filler Effect: The Influence of Filler Content and Surface Area on Cementitious Reaction Rates, J Am Ceram Soc, 96 (2013) 1978 - 1990. [389] E.H. Oelkers, General kinetic description of multioxide silicate mineral and glass dissolution, Geochimica et Cosmochimica Acta, 65 (2001) 3703-3719. [390] J.J. Thomas, H.M. Jennings, A colloidal interpretation of chemical aging of the C-S-H gel and its effects on the properties of cement paste, Cement and Concrete Research, 36 (2006) 30-38. [391] G.J. Stockmann, D. Wolff-Boenisch, N. Bovet, S.R. Gislason, E.H. Oelkers, The role of silicate surfaces on calcite precipitation kinetics, Geochimica et Cosmochimica Acta, 135 (2014) 231-250. [392] N. Voglis, G. Kakali, E. Chaniotakis, S. Tsivilis, Portland-limestone cements. Their properties and hydration compared to those of other composite cements, Cement and Concrete Composites, 27 (2005) 191-196. [393] M. Ben Haha, B. Lothenbach, G. Le Saout, F. Winnefeld, Influence of slag chemistry on the hydration of alkali-activated blast-furnace slag — Part I: Effect of MgO, Cement and Concrete Research, 41 (2011) 955-963. [394] O. Chowaniec, Limestone addition in cement., in: Laboratoire des matériaux de construction, EPFL, 2012. [395] L. Montanaro, A. Negro, M. Regourd, Action de CaCO3, CaSO4 et CaSO4· 2H2O sur l'Hydratation de C3S, Cement and Concrete Research, 18 (1988) 431-437. [396] A.P. Barker, An electron optical examination of zoning in blastfurnace slag hydrates: Part I. Slag cement pastes at early ages, Advances in Cement Research, 2 (1989) 171-179. [397] A. Vollpracht, B. Lothenbach, R. Snellings, J. Haufe, The pore solution of blended cements: a review, Materials and Structures, 49 (2016) 3341-3367. [398] D.-T. Nguyen, R. Alizadeh, J.J. Beaudoin, L. Raki, Microindentation creep of secondary hydrated cement phases and C–S–H, Materials and Structures, 46 (2013) 1519-1525. [399] EN206:2013, Concrete. Specification, performance, production and conformity, in, 2013. [400] C. Hall, Water sorptivity of mortars and concretes: a review, Magazine of Concrete Research, 41 (1989) 51-61. [401] M. Ghirci, S. Kenai, M. Said-Mansour, Mechanical properties and durability of mortar and concrete containing natural pozzolana and limestone blended cements, Cement and Concrete Composites, 29 (2007) 542-549. [402] V. Bonavetti, V. Rahhal, E.F. Irassar, Studies on the carboaluminate formation in limestone filler-blended cements, Cement and Concrete Research, 31 (2001) 853-859. [403] DDCEN/TS12390-9:2006, Testing hardened concrete. Freeze-thaw resistance. Scaling, in. [404] S. Rahman, Z. Grasley, E. Masad, D. Zollinger, S. Iyengar, R. Kogbara, Simulation of Mass, Linear Momentum, and Energy Transport in Concrete with Varying Moisture Content during Cooling to Cryogenic Temperatures, Transport in Porous Media, 112 (2016) 139-166. [405] H. Cai, X. Liu, Freeze-thaw durability of concrete: ice formation process in pores, Cement and Concrete Research, 28 (1998) 1281-1287. [406] T. RILEM, L.T. IDC, P. P-E, Final Recommendation of RILEM TC 176-IDC'Internal Damage of Concrete due to frost action', Materials and Structures, 37 (2004) 754-759. [407] P.A.M. Basheer, # Clam'permeability tests for assessing the durability of concrete, in, Queen's University of Belfast, 1991. [408] G. Fagerlund, The critical degree of saturation method of assessing the freeze/thaw resistance of concrete, Matériaux et Construction, 10 (1977) 217-229. [409] Z. Liu, W. Hansen, A hypothesis for salt frost scaling in cementitious materials, Journal of Advanced Concrete Technology, 13 (2015) 403-414. [410] Z. Liu, W. Hansen, Freezing characteristics of air-entrained concrete in the presence of deicing salt, Cement and Concrete Research, 74 (2015) 10-18. [411] S. Tsivilis, G. Batis, E. Chaniotakis, G. Grigoriadis, D. Theodossis, Properties and behavior of limestone cement concrete and mortar, Cement and Concrete Research, 30 (2000) 1679-1683. [412] A. Morandeau, M. Thiéry, P. Dangla, Impact of accelerated carbonation on OPC cement paste blended with fly ash, Cement and Concrete Research, 67 (2015) 226-236. [413] K. Suzuki, T. Nishikawa, S. Ito, Formation and carbonation of C-S-H in water, Cement and Concrete Research, 15 (1985) 213-224. [414] F. Sanchez, M.K. Langley White, A. Hoang, Leaching from granular cement-based materials during infiltration/wetting coupled with freezing and thawing, Journal of Environmental Management, 90 (2009) 983-993. [415] C. Carde, R. François, J.-M. Torrenti, Leaching of both calcium hydroxide and C-S-H from cement paste: Modeling the mechanical behavior, Cement and Concrete Research, 26 (1996) 1257-1268. [416] C. Gervais, A.C. Garrabrants, F. Sanchez, R. Barna, P. Moszkowicz, D.S. Kosson, The effects of carbonation and drying during intermittent leaching on the release of inorganic constituents from a cement-based matrix, Cement and Concrete Research, 34 (2004) 119-131. [417] T. Nishikawa, K. Suzuki, S. Ito, K. Sato, T. Takebe, Decomposition of synthesized ettringite by carbonation, Cement and Concrete Research, 22 (1992) 6-14. [418] A. Hidalgo, C. Domingo, C. Garcia, S. Petit, C. Andrade, C. Alonso, Microstructural changes induced in Portland cement-based materials due to natural and supercritical carbonation, Journal of Materials Science, 43 (2008) 3101-3111. [419] S.A. Bernal, M.C. Juenger, X. Ke, W. Matthes, B. Lothenbach, N. De Belie, J.L. Provis, Characterization of supplementary cementitious materials by thermal analysis, Materials and Structures, 50 (2017) 26. [420] L. Divet, R. Randriambololona, Delayed Ettringite Formation: The Effect of Temperature and Basicity on the Interaction of Sulphate and C-S-H Phase 1, Cement and Concrete Research, 28 (1998) 357-363. [421] J.J. Thomas, J.J. Chen, A.J. Allen, H.M. Jennings, Effects of decalcification on the microstructure and surface area of cement and tricalcium silicate pastes, Cement and Concrete Research, 34 (2004) 2297-2307. [422] J.E. Rossen, B. Lothenbach, K.L. Scrivener, Composition of C–S–H in pastes with increasing levels of silica fume addition, Cement and Concrete Research, 75 (2015) 14-22. [423] R.K. Iler, Effect of adsorbed alumina on the solubility of amorphous silica in water, Journal of Colloid and Interface Science, 43 (1973) 399-408. [424] L. Lam, Y.L. Wong, C.S. Poon, Degree of hydration and gel/space ratio of high-volume fly ash/cement systems, Cement and Concrete Research, 30 (2000) 747-756."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.714270"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/17446/1/The%20Relationship%20between%20composition%20microstructure%20and%20performance%20of%20composite%20cements-Corrected.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Cement production is a major contributor to anthropogenic CO2 emissions. Composite slag cement is one way of reducing the clinker factor, and hence emissions. Synergies between limestone and slag have been suggested to enhance the performance of such cement. The synergistic effect on mechanical performance has been ascribed to the carboalumination formation, which in turn prevents the conversion of ettringite to mono sulphoaluminate. Whilst the benefits of the synergy are documented, causation factors are not fully understood. In order to maximise the synergy, a clear understanding of the relationship between composition and the carboalumination-ettringite balance and how this impacts on performance is essential. Consequently, this study focused on the kinetics of reaction, microstructure and the implications on strength development and the freeze-thaw durability. The QXRD/PONKCS method proposed elsewhere has been extended to monitor the residual slag contents in ternary blended systems. The slag phase was modelled from the x-ray diffraction pattern of a 100 % slag specimen. The model was then calibrated on a 50:50 mixture of slag and corundum using the internal standard method. The measurement accuracy was found to be ± 2 % following implementation of the calibrated slag phase on simplified slag-corundum mixes of varying proportions. In hydrated cement systems, however, the accuracy established from the comparison between the results from QXRD/PONKCS and SEM/IA analysis was ± 6 %. The investigated hydration stopping methods except freeze-drying had minimal impact on the results as long as the mass attenuation coefficient (MAC) was accurately quantified. For implementing the QXRD/PONKCS method, freshly ground non-hydration stopped sample preparation is recommended. This method presented the least challenge in calculating the MAC and also preserve the other hydrates particularly the AFt/AFm phases. However, if hydration stopping cannot be avoided, a double solvent exchange regime using isopropanol and diethyl ether is recommended. The residual slag content is overestimated from freeze-dried samples. Multiple techniques including the QXRD/PONKCS method, SEM/IA, isothermal conduction calorimetry, chemical shrinkage and thermal analysis were subsequently used to investigate the kinetics of hydration. These revealed that limestone accelerates slag and clinker hydration. Alite hydration is accelerated by the supplementary cementitious materials including slag and quartz. However, while belite hydration is retarded in the binary slag mix, this is not the case in limestone ternary blends. Calcium carbonate also reacts with additionally dissolved aluminates instead of the latter converting ettringite to mono sulphoaluminate. Therefore, the synergy between limestone and slag is not only due to preserved ettringite but the additional hydrates and pore structure modification. The carboaluminate content is higher in the presence of limestone but the home to mono carboaluminate balance shifts with the limestone content. The aluminates available for incorporation into other hydrates and in the pore solution are lowered by carboaluminate formation. The pore structure and pore solution chemistry were analysed in order to further investigate the mechanisms for the accelerated dissolution of slag and the major clinker phases. The overall pore volumes as measured by MIP were similar in the slag containing mixes with or without limestone. Evaluation of the free water content at the end of experiment also indicated excess free water thus indicating that the pore structure and capillary pore water are not the limiting factors for slag hydration in the investigated mixes. The identified drivers behind the role of limestone in the synergy are the nucleation and dilution effects in the case of clinker, while for slag hydration pore solution effects are important. The incorporation of alumina into carboaluminates and C-S-H lowers the alumina in the pore solution and consequently promote slag dissolution. The freeze-thaw resistance of the ternary blends at the investigated 0.5 water/binder ratio is low compared to the CEM I 42.5 R concrete. Decalcification through carbonation during conditioning and leaching during freeze-thaw is identified to be the dominant microstructural difference between degraded and non-degraded samples. A chemo-mechanical degradation mechanism, which is similar to the glue-spall mechanism, is hypothesised for surface scaling during freeze-thaw. By this, freeze-thaw damage in concrete is caused by decalcification and spalling of successive layers under induced stresses of ice growth."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Relationship between Microstructure, Durability and Performance of CEM X Composite Cements"]}]}],"canonical_facts":{"dc:contributor.advisor":["Black, Leon"],"dc:contributor.sponsor":["University of Leeds","Heidelberg Technology Centre"],"dc:creator":["Adu-Amankwah, Samuel"],"dc:date":["2016-10-31"],"dc:date.issued":["2016-10"],"dc:description.abstract":["Cement production is a major contributor to anthropogenic CO2 emissions. Composite slag cement is one way of reducing the clinker factor, and hence emissions. Synergies between limestone and slag have been suggested to enhance the performance of such cement. The synergistic effect on mechanical performance has been ascribed to the carboalumination formation, which in turn prevents the conversion of ettringite to mono sulphoaluminate. Whilst the benefits of the synergy are documented, causation factors are not fully understood. In order to maximise the synergy, a clear understanding of the relationship between composition and the carboalumination-ettringite balance and how this impacts on performance is essential. Consequently, this study focused on the kinetics of reaction, microstructure and the implications on strength development and the freeze-thaw durability. The QXRD/PONKCS method proposed elsewhere has been extended to monitor the residual slag contents in ternary blended systems. The slag phase was modelled from the x-ray diffraction pattern of a 100 % slag specimen. The model was then calibrated on a 50:50 mixture of slag and corundum using the internal standard method. The measurement accuracy was found to be ± 2 % following implementation of the calibrated slag phase on simplified slag-corundum mixes of varying proportions. In hydrated cement systems, however, the accuracy established from the comparison between the results from QXRD/PONKCS and SEM/IA analysis was ± 6 %. The investigated hydration stopping methods except freeze-drying had minimal impact on the results as long as the mass attenuation coefficient (MAC) was accurately quantified. For implementing the QXRD/PONKCS method, freshly ground non-hydration stopped sample preparation is recommended. This method presented the least challenge in calculating the MAC and also preserve the other hydrates particularly the AFt/AFm phases. However, if hydration stopping cannot be avoided, a double solvent exchange regime using isopropanol and diethyl ether is recommended. The residual slag content is overestimated from freeze-dried samples. Multiple techniques including the QXRD/PONKCS method, SEM/IA, isothermal conduction calorimetry, chemical shrinkage and thermal analysis were subsequently used to investigate the kinetics of hydration. These revealed that limestone accelerates slag and clinker hydration. Alite hydration is accelerated by the supplementary cementitious materials including slag and quartz. However, while belite hydration is retarded in the binary slag mix, this is not the case in limestone ternary blends. Calcium carbonate also reacts with additionally dissolved aluminates instead of the latter converting ettringite to mono sulphoaluminate. Therefore, the synergy between limestone and slag is not only due to preserved ettringite but the additional hydrates and pore structure modification. The carboaluminate content is higher in the presence of limestone but the home to mono carboaluminate balance shifts with the limestone content. The aluminates available for incorporation into other hydrates and in the pore solution are lowered by carboaluminate formation. The pore structure and pore solution chemistry were analysed in order to further investigate the mechanisms for the accelerated dissolution of slag and the major clinker phases. The overall pore volumes as measured by MIP were similar in the slag containing mixes with or without limestone. Evaluation of the free water content at the end of experiment also indicated excess free water thus indicating that the pore structure and capillary pore water are not the limiting factors for slag hydration in the investigated mixes. The identified drivers behind the role of limestone in the synergy are the nucleation and dilution effects in the case of clinker, while for slag hydration pore solution effects are important. The incorporation of alumina into carboaluminates and C-S-H lowers the alumina in the pore solution and consequently promote slag dissolution. The freeze-thaw resistance of the ternary blends at the investigated 0.5 water/binder ratio is low compared to the CEM I 42.5 R concrete. Decalcification through carbonation during conditioning and leaching during freeze-thaw is identified to be the dominant microstructural difference between degraded and non-degraded samples. A chemo-mechanical degradation mechanism, which is similar to the glue-spall mechanism, is hypothesised for surface scaling during freeze-thaw. By this, freeze-thaw damage in concrete is caused by decalcification and spalling of successive layers under induced stresses of ice growth."],"dc:format":["text"],"dc:identifier":["uk.bl.ethos.714270"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/17446/1/The%20Relationship%20between%20composition%20microstructure%20and%20performance%20of%20composite%20cements-Corrected.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.commercial":["University of Leeds"],"dc:publisher.department":["Faculty of Engineering (Leeds)","School of Civil Engineering (Leeds)"],"dc:publisher.institution":["University of Leeds"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/17446/"],"dc:relation.references":["List of References [1] J.S. Damtoft, J. Lukasik, D. Herfort, D. Sorrentino, E.M. Gartner, Sustainable development and climate change initiatives, Cement and Concrete Research, 38 (2008) 115-127. [2] ECOBA, European Coal Ash Unitlisation, in, 2016. [3] J.A. Ober, Mineral commodity summaries 2016, in, US Geological Survey, 2016. [4] V. Bonavetti, H. Donza, V. Rahhal, E. Irassar, Influence of initial curing on the properties of concrete containing limestone blended cement, Cement and Concrete Research, 30 (2000) 703-708. [5] R. Hooton, M. Nokken, M. Thomas, Portland-limestone cement: state-of-the-art report and gap analysis for CSA A 3000, Cement Association of Canada University of Toronto, (2007). [6] P.D. Tennis, M.D.A. Thomas, W.J. Weiss, State-of-the-Art Report on Use of Limestone in Cements at Levels of up to 15%, in, Portland Cement Association, Skokie, Illinois, 2011, pp. 78. [7] K. De Weerdt, M. Ben Haha, G. Le Saout, K.O. Kjellsen, H. Justnes, B. Lothenbach, Hydration mechanisms of ternary Portland cements containing limestone powder and fly ash, Cement and Concrete Research, 41 (2011) 279-291. [8] G. Menéndez, V. Bonavetti, E.F. Irassar, Strength development of ternary blended cement with limestone filler and blast-furnace slag, Cement and Concrete Composites, 25 (2003) 61-67. [9] M. Moesgaard, S.L. Poulsen, D. Herfort, M. Steenberg, L.K. Kirkegaard, J. Skibsted, Y. Yue, Hydration of Blended Portland Cements Containing Calcium-Aluminosilicate Glass Powder and Limestone, Journal of the American Ceramic Society, 95 (2012) 403–409. [10] B. Lothenbach, K. Scrivener, R.D. Hooton, Supplementary cementitious materials, Cement and Concrete Research, 41 (2011) 1244-1256. [11] X. Wu, W. Jiang, D.M. Roy, Early activation and properties of slag cement, Cement and Concrete Research, 20 (1990) 961-974. [12] J.I. Escalante, L.Y. Gómez, K.K. Johal, G. Mendoza, H. Mancha, J. Méndez, Reactivity of blast-furnace slag in Portland cement blends hydrated under different conditions, Cement and Concrete Research, 31 (2001) 1403-1409. [13] J. Cailetti, A.M. Soliman, M.L. Nehdi, Effects of nano- and micro-limestone addition on early-age properties of ultra-high-performance concrete, Materials and Structures, 46 (2013) 881-898. [14] S. Hoshino, K. Yamada, H. Hirao, XRD/Rietveld analysis of the hydration and strength development of slag and limestone blened cement, Advanced Concrete Technology, 4 (2006) 357-367. [15] S. Ogawa, T. Nozaki, K. Yamada, H. Hirao, R.D. Hooton, Improvement on sulfate resistance of blended cement with high alumina slag, Cement and Concrete Research, 42 (2012) 244-251. [16] S. Tsivilis, E. Chaniotakis, E. Badogiannis, G. Pahoulas, A. Ilias, A study on the parameters affecting the properties of Portland limestone cements, Cement and Concrete Composites, 21 (1999) 107-116. [17] B. Lothenbach, G. Le Saout, E. Gallucci, K. Scrivener, Influence of limestone on the hydration of Portland cements, Cement and Concrete Research, 38 (2008) 848-860. [18] M. Moesgaard, D. Herfort, M. Steenberg, L.F. Kirkegaard, Y. Yue, Physical performances of blended cements containing calcium aluminosilicate glass powder and limestone, Cement and Concrete Research, 41 (2011) 359-364. [19] A.M. Ramezanianpour, R.D. Hooton, Sulfate resistance of Portland-limestone cements in combination with supplementary cementitious materials, Materials and Structures, 46 (2012) 1061-1073 [20] T. Schmidt, B. Lothenbach, M. Romer, J. Neuenschwander, K. Scrivener, Physical and microstructural aspects of sulfate attack on ordinary and limestone blended Portland cements, Cement and Concrete Research, 39 (2009) 1111-1121. [21] K.u. Githachuri, M.G. Alexander, Durability performance potential and strength of blended Portland limestone cement concrete, Cement and Concrete Composites, 39 (2013) 115-121. [22] B. Persson, Internal frost resistance and salt frost scaling of self-compacting concrete, Cement and Concrete Research, 33 (2003) 373-379. [23] S. Grzeszczyk, P. Podkowa, The Effect of Limestone Filler on the Properties of Self Compacting Concrete, ANNUAL TRANSACTIONS OF THE NORDIC RHEOLOGY SOCIETY, , VOL. 17 (2009). [24] R.K. Dhir, M.C. Limbachiya, M.J. Macarthy, A. Chaipanich, Evaluation of Portland limestone cements for use in concrete construction, Materials and Structures, 40 (2007) 459 - 473. [25] J. Stark, H.M. Ludwig, Freeze-deicing salt resistance of concretes containing cement rich in slag, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop, E & FN SPON, University of Essen, 1997, pp. 123-138. [26] B. Espion, B. Lebon, O. Germain, A. Hellebois, Characterisation of new ternary cements with reduced clinker content in: K. Sakai (Ed.) Proceedings of the First International Conference on Concrete Sustainability, Tokyo, Japan, 2013, pp. 145 - 152. [27] M. Collepardi, S. Collepardi, J.J. Ogoumah Olagot, E. Simonelli, The Influence of Slag and Fly Ash on the Carbonation, in: V.M. Malhotra (Ed.) Eighth CANMET/ACI International Conference on Fly Ash, Silica Fume, Slag, and Natural Pozzolans in Concrete 2004. [28] M. Ben Haha, K. De Weerdt, B. Lothenbach, Quantification of the degree of reaction of fly ash, Cement and Concrete Research, 40 (2010) 1620-1629. [29] V. Kocaba, E. Gallucci, K.L. Scrivener, Methods for determination of degree of reaction of slag in blended cement pastes, Cement and Concrete Research, 42 (2012) 511-525. [30] K. Luke, F.P. Glasser, Selective dissolution of hydrated blast furnace slag cements, Cement and Concrete Research, 17 (1987) 273-282. [31] M. Whittaker, M. Zajac, M. Ben Haha, F. Bullergahn, L. Black, The role of the alumina content of slag, plus the presence of additional sulfate on the hydration and microstructure of Portland cement-slag blends, Cement and Concrete Research, 66 (2014) 91-101. [32] N.V.Y. Scarlett, I.C. Madsen, Quantification of phases with partial or no known crystal structures, Powder Diffraction, 21 (2006) 278-284. [33] R. Snellings, A. Salze, K.L. Scrivener, Use of X-ray diffraction to quantify amorphous supplementary cementitious materials in anhydrous and hydrated blended cements, Cement and Concrete Research, 64 (2014) 89-98. [34] J. Marchand, Y. Maltais, Y. Machabee, C. TAlbot, M. Pigeon, Effects of fly ash on microstructure and deicer salt scaling resistance of concrete, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop, University of Essen, 1997, pp. 11 - 20. [35] J.J. Valenza Ii, G.W. Scherer, A review of salt scaling: II. Mechanisms, Cement and Concrete Research, 37 (2007) 1022-1034. [36] J.J. Valenza, G.W. Scherer, A review of salt scaling: I. Phenomenology, Cement and Concrete Research, 37 (2007) 1007-1021. [37] T.C. Powers, A Working Hypothesis for Further Studies of Frost Resistance of Concrete, ACI Journal Proceedings, 41 (1945) 245-272. [38] T.C. Powers, R.A. Helmuth, Theory of volume changes in hardened Portland cement paste during freezing, Highway Research Board, 32 (1953). [39] G.W. Scherer, Crystallization in pores, Cement and Concrete Research, 29 (1999) 1347-1358. [40] G.W. Scherer, J. Valenza, Mechanisms of frost damage, Materials science of concrete, 7 (2005) 209-246. [41] P.-w. Gao, S.-x. Wu, P.-h. Lin, Z.-r. Wu, M.-s. Tang, The characteristics of air void and frost resistance of RCC with fly ash and expansive agent, Construction and Building Materials, 20 (2006) 586-590. [42] G.-F. Peng, Q. Ma, H.-M. Hu, R. Gao, Q.-F. Yao, Y.-F. Liu, The effects of air entrainment and pozzolans on frost resistance of 50–60&#xa0;MPa grade concrete, Construction and Building Materials, 21 (2007) 1034-1039. [43] K. Fridh, Internal frost damage in concrete - experimental studies of destruction mechanisms, in: Division of Building Materials, University of Lund, 2005. [44] J. Deja, Freezing and de-icing salt resistance of blast furnace slag concretes, Cement and Concrete Composites, 25 (2003) 357-361. [45] D.J. Janssen, M.B. Snyder, Resistance of concrete to freezing and thawing, 1994. [46] K.L. Scrivener, Backscattered electron imaging of cementitious microstructures: understanding and quantification, Cement and Concrete Composites, 26 (2004) 935-945. [47] R.J. Detwiler, B.J. Dalgleish, R.B. Williamson, Assessing the durability of concrete in freezing and thawing, ACI Materials Journal, 86 (1989) 29-35. [48] M. Tang, Y. Tian, X.B. Mu, M. Jiang, The Pore Fractal Characteristics of Concrete Materials under Salt Freezing Conditions in Cold Area, Advanced Materials Research, 233 - 235 (2011) 2522 - 2527. [49] N.V. Scarlett, I.C. Madsen, Current state of quantitative phase analysis, in: Accuracy in Powder Diffraction, APD-IV, 2013. [50] E. Gartner, Industrially interesting approaches to “low-CO2” cements, Cement and Concrete Research, 34 (2004) 1489-1498. [51] E. Berodier, K. Scrivener, Understanding the filler effect on the nucleation and growth of C-S-H, Journal of the American Ceramic Society, 97 (2014) 3764-3773. [52] F. Deschner, F. Winnefeld, B. Lothenbach, S. Seufert, P. Schwesig, S. Dittrich, F. Goetz-Neunhoeffer, J. Neubauer, Hydration of Portland cement with high replacement by siliceous fly ash, Cement and Concrete Research, 42 (2012) 1389-1400. [53] K.L. Scrivener, P. Juilland, P.J.M. Monteiro, Advances in understanding hydration of Portland cement, Cement and Concrete Research, 78, Part A (2015) 38-56. [54] E. Berodier, K. Scrivener, Evolution of pore structure in blended systems, Cement and Concrete Research, 73 (2015) 25-35. [55] B. Lothenbach, G. Le Saout, M. Ben Haha, R. Figi, E. Wieland, Hydration of a low-alkali CEM III/B–SiO2 cement (LAC), Cement and Concrete Research, 42 (2012) 410-423. [56] CEMBUREAU, Environmental benefits of using alternative fuels in cement production: A life-cycle approach, in, The European Cement Association, 2010. [57] G. Habert, C. Billard, P. Rossi, C. Chen, N. Roussel, Cement production technology improvement compared to factor 4 objectives, Cement and Concrete Research, 40 (2010) 820-826. [58] G.P. Hammond, C.I. Jones, Embodied energy and carbon in construction materials, Proc Institution of Civil Engineers: Energy, (2008). [59] Ernst Worrell, Lynn Price, Nathan Martin, Chris Hendriks, L.O. Meida, Carbon dioxide emissions from the global cement industry, Annual Review of Energy and the Environment, 26 (2001) 303-329. [60] P. Mehta, H. Meryman, Tools for Reducing Carbon Emissions Due to Cement Consumption, Structure Magazine, (2009) 11-15. [61] P. Purnell, L. Black, Embodied carbon dioxide in concrete: Variation with common mix design parameters, Cement and Concrete Research, 42 (2012) 874-877. [62] J.H. Sharp, E.M. Gartner, D.E. Macphee, Novel cement systems (sustainability). Session 2 of the Fred Glasser Cement Science Symposium, Advances in Cement Research, 22 (2010) 195-202. [63] A. Palomo, M.W. Grutzeck, M.T. Blanco, Alkali-activated fly ashes: A cement for the future, Cement and Concrete Research, 29 (1999) 1323-1329. [64] F. Winnefeld, B. Lothenbach, Hydration of calcium sulfoaluminate cements — Experimental findings and thermodynamic modelling, Cement and Concrete Research, 40 (2010) 1239-1247. [65] Y. Li, B. Chen, Factors that affect the properties of magnesium phosphate cement, Construction and Building Materials, 47 (2013) 977-983. [66] J.W. Phair, Green chemistry for sustainable cement production and use, Green Chemistry, 8 (2006) 763-780. [67] K. Scrivener, B. Lothenbach, N. De Belie, E. Gruyaert, J. Skibsted, R. Snellings, A. Vollpracht, TC 238-SCM: hydration and microstructure of concrete with SCMs, Materials and Structures, 48 (2015) 835-862. [68] E. Badogiannis, S. Tsivilis, Exploitation of poor Greek kaolins: Durability of metakaolin concrete, Cement and Concrete Composites, 31 (2009) 128-133. [69] T.W. Cheng, J.P. Chiu, Fire-resistant geopolymer produced by granulated blast furnace slag, Minerals Engineering, 16 (2003) 205-210. [70] K.L. Scrivener, J.-L. Cabiron, R. Letourneux, High-performance concretes from calcium aluminate cements, Cement and Concrete Research, 29 (1999) 1215-1223. [71] J. Bensted, Calcium aluminate cements, in: J.Bensted, P.Barnes (Eds.) Structure and Performance of Cements, SPON Press, 2002, pp. 114-138. [72] K. Scrivener, Calcium aluminate cements, in: J. Newman, B.S. Choo (Eds.) Advanced Concrete Technology 1: Constituent Materials, Butterworth-Heinemann, 2003, pp. 2/1-2/29. [73] F.P. Glasser, L. Zhang, High-performance cement matrices based on calcium sulfoaluminate–belite compositions, Cement and Concrete Research, 31 (2001) 1881-1886. [74] K. Quillin, Performance of belite–sulfoaluminate cements, Cement and Concrete Research, 31 (2001) 1341-1349. [75] J.L. Provis, Geopolymers and other alkali activated materials: why, how, and what?, Materials and Structures, 47 (2014) 11-25. [76] S.A. Bernal, J.L. Provis, R.J. Myers, R. San Nicolas, J.S. van Deventer, Role of carbonates in the chemical evolution of sodium carbonate-activated slag binders, Materials and Structures, 48 (2015) 517-529. [77] P. Duxson, A. Fernández-Jiménez, J.L. Provis, G.C. Lukey, A. Palomo, J.S.J. van Deventer, Geopolymer technology: the current state of the art, Journal of Materials Science, 42 (2007) 2917-2933. [78] A. Fernández-Jiménez, A. Palomo, Composition and microstructure of alkali activated fly ash binder: Effect of the activator, Cement and Concrete Research, 35 (2005) 1984-1992. [79] A. Fernández-Jiménez, A. Palomo, M. Criado, Microstructure development of alkali-activated fly ash cement: a descriptive model, Cement and Concrete Research, 35 (2005) 1204-1209. [80] B.C. McLellan, R.P. Williams, J. Lay, A. Van Riessen, G.D. Corder, Costs and carbon emissions for geopolymer pastes in comparison to ordinary Portland cement, Journal of Cleaner Production, 19 (2011) 1080-1090. [81] D.N. Huntzinger, T.D. Eatmon, A life-cycle assessment of Portland cement manufacturing: comparing the traditional process with alternative technologies, Journal of Cleaner Production, 17 (2009) 668-675. [82] H.F.W. Taylor, Nanostructure of CSH: Current status, Advanced Cement Based Materials, 1 (1993) 38-46. [83] H.F.W. Taylor, Cement Chemistry, 2nd ed., Thomas Telford, 1997. [84] N.L. Thomas, D.D. Double, The hydration of Portland cement, C3S and C2S in the presence of a calcium complexing admixture (EDTA), Cement and Concrete Research, 13 (1983) 391-400. [85] P. Barret, D. Ménétrier, Filter dissolution of C3S as a function of the lime concentration in a limited amount of lime water, Cement and Concrete Research, 10 (1980) 521-534. [86] J.W. Bullard, H.M. Jennings, R.A. Livingston, A. Nonat, G.W. Scherer, J.S. Schweitzer, K.L. Scrivener, J.J. Thomas, Mechanisms of cement hydration, Cement and Concrete Research, 41 (2011) 1208-1223. [87] H.F.W. Taylor, P. Barret, P.W. Brown, D.D. Double, G. Frohnsdorff, V. Johansen, D. Ménétrier-Sorrentino, I. Odler, L.J. Parrott, J.M. Pommersheim, M. Regourd, J.F. Young, The hydration of tricalcium silicate, Matériaux et Construction 17 (1984) 457-468 [88] S. Mindess, J.F. Young, D. Darwin, Concrete, Prentice Hall PTR, 2003. [89] D. Stephan, S. Wistuba, Crystal structure refinement and hydration behaviour of 3CaO·SiO2 solid solutions with MgO, Al2O3 and Fe2O3, Journal of the European Ceramic Society, 26 (2006) 141-148. [90] M. Bigare, A. Guinier, C. Mazieres, M. Regourd, N. YannaquisS, W. Eysbl, T. HahnA, E. Woermann, Polymorphism of Tricalcium Silicate and Its Solid Solutions, Journal of the American Ceramic Society, 50 (1967) 609-619. [91] S. Ma, W. Zhou, S. Wang, W. Li, X. Shen, Polymorph transformation kinetics of Ca3SiO5 with MgO, Phase Transitions, 88 (2015) 888-896. [92] M.-N. de Noirfontaine, M. Courtial, F. Dunstetter, G. Gasecki, M. Signes-Frehel, Tricalcium silicate Ca3SiO5 superstructure analysis: a route towards the structure of the M1 polymorph, in: Zeitschrift für Kristallographie Crystalline Materials, 2012, pp. 102. [93] F. Dunstetter, M.N. de Noirfontaine, M. Courtial, Polymorphism of tricalcium silicate, the major compound of Portland cement clinker: 1. Structural data: review and unified analysis, Cement and Concrete Research, 36 (2006) 39-53. [94] I. Odler, Hydration, Setting and Hardening of Portland Cement in: Lea’s Chemistry of Cement&Concrete, Butterworth Heinemann, Oxford, 2001, pp. 241. [95] S. Abdul-Maula, I. Odler, Structure and properties of tricalcium silicate doped with MgO, Al 2 O 3 and Fe 2 O 3, in: Proc Br Ceram Soc, 1984, pp. 83. [96] D. Stephan, S.N. Dikoundou, G. Raudaschl-Sieber, Hydration characteristics and hydration products of tricalcium silicate doped with a combination of MgO, Al2O3 and Fe2O3, Thermochimica Acta, 472 (2008) 64-73. [97] G.L. Valenti, V. Sabatelli, B. Marchese, Hydration kinetics of tricalcium silicate solid solutions at early ages, Cement and Concrete Research, 8 (1978) 61-72. [98] I.a. Odler, S. Abdul-Maula, Polymorphism and Hydration of Tricalcium Silicate Doped With ZnO, Journal of the American Ceramic Society, 66 (1983) 1-4. [99] H.R. Stewart, J.E. Bailey, Microstructural studies of the hydration products of three tricalcium silicate polymorphs, Journal of Materials Science, 18 (1983) 3686-3694. [100] A. Bazzoni, S. Ma, Q. Wang, X. Shen, M. Cantoni, K.L. Scrivener, The Effect of Magnesium and Zinc Ions on the Hydration Kinetics of C3S, Journal of the American Ceramic Society, 97 (2014) 3684-3693. [101] T. Staněk, P. Sulovský, The influence of the alite polymorphism on the strength of the Portland cement, Cement and Concrete Research, 32 (2002) 1169-1175. [102] L. Fernandez, C. Alonso, A. Hidalgo, C. Andrade, The role of magnesium during the hydration of C3S and CSH formation. Scanning electron microscopy and mid-infrared studies, Advances in cement research, 17 (2005) 9-21. [103] I.G. Richardson, G.W. Groves, Microstructure and microanalysis of hardened ordinary Portland cement pastes, Journal of Materials Science, 28 (1993) 265-277. [104] I.G. Richardson, A.R. Brough, R. Brydson, G.W. Groves, C.M. Dobson, Location of Aluminum in Substituted Calcium Silicate Hydrate (C-S-H) Gels as Determined by 29Si and 27Al NMR and EELS, Journal of the American Ceramic Society, 76 (1993) 2285 - 2286. [105] C. Tashiro, S. Tatibana, Bond strength between C3S paste and iron, copper or zinc wire and microstructure of interface, Cement and Concrete Research, 13 (1983) 377-382. [106] D. Jansen, S.T. Bergold, F. Goetz-Neunhoeffer, J. Neubauer, The hydration of alite: a time-resolved quantitative X-ray diffraction approach using the G-factor method compared with heat release, J Appl Cryst, 44 (2011) 895-901. [107] D. Jansen, F. Goetz-Neunhoeffer, B. Lothenbach, J. Neubauer, The early hydration of Ordinary Portland Cement (OPC): An approach comparing measured heat flow with calculated heat flow from QXRD, Cement and Concrete Research, 42 (2012) 134-138. [108] J.B. Ings, P.W. Brown, G. Frohnsdorff, Early hydration of large single crystals of tricalcium silicate, Cement and Concrete Research, 13 (1983) 843-848. [109] J.J. Thomas, H.M. Jennings, J.J. Chen, Influence of Nucleation Seeding on the Hydration Mechanisms of Tricalcium Silicate and Cement, The Journal of Physical Chemistry, 113 (2009) 4327-4334. [110] A. Comotti, G. Castaldi, C. Gilioli, G. Torri, P. Sozzani, Step-by-step observation of the hydration of C3S by magic-angle spinning 29Si nuclear magnetic resonance: the masking effect of D2O, Journal of Materials Science, 29 (1994) 6427-6433. [111] J.J. Thomas, S.A. FitzGerald, D.A. Neumann, R.A. Livingston, State of Water in Hydrating Tricalcium Silicate and Portland Cement Pastes as Measured by Quasi-Elastic Neutron Scattering, Journal of the American Ceramic Society, 84 (2001) 1811-1816. [112] E. Pustovgar, R.P. Sangodkar, A.S. Andreev, M. Palacios, B.F. Chmelka, R.J. Flatt, J.-B. d/'Espinose de Lacaillerie, Understanding silicate hydration from quantitative analyses of hydrating tricalcium silicates, Nat Commun, 7 (2016). [113] E.M. Gartner, Hydration mechanisms I, American Ceramic Society, 1 (1989) 95-125. [114] P. Juilland, E. Gallucci, R. Flatt, K. Scrivener, Dissolution theory applied to the induction period in alite hydration, Cement and Concrete Research, 40 (2010) 831-844. [115] A. Nonat, The structure and stoichiometry of C-S-H, Cement and Concrete Research, 34 (2004) 1521-1528. [116] E.M. Gartner, H.M. Jennings, Thermodynamics of calcium silicate hydrates and their solutions, J Am Ceram Soc 80 (1987) 743–749. [117] H.N. Stein, J.M. Stevels, Influence of silica on the hydration of 3 CaO,SiO2, Journal of Applied Chemistry, 14 (1964) 338-346. [118] H.M. Jennings, P.L. Pratt, An experimental argument for the existence of a protective membrane surrounding portland cement during the induction period, Cement and Concrete Research, 9 (1979) 501-506. [119] S. Garrault, T. Behr, A. Nonat, Formation of the C−S−H Layer during Early Hydration of Tricalcium Silicate Grains with Different Sizes, The Journal of Physical Chemistry B, 110 (2006) 270-275. [120] S. Garrault, E. Finot, E. Lesniewska, A. Nonat, Study of C-S-H growth on C3S surface during its early hydration, Materials and Structures, 38 (2005) 435-442. [121] F. Tzschichholz, H. Zanni, Global hydration kinetics of tricalcium silicate cement, Physical Review E, 64 (2001) 016115. [122] A. Kumar, S. Bishnoi, K.L. Scrivener, Modelling early age hydration kinetics of alite, Cement and Concrete Research, 42 (2012) 903-918. [123] A.K. Chatterjee, High belite cements—Present status and future technological options: Part I, Cement and Concrete Research, 26 (1996) 1213-1225. [124] J.G. Jang, H.K. Lee, Microstructural densification and CO2 uptake promoted by the carbonation curing of belite-rich Portland cement, Cement and Concrete Research, 82 (2016) 50-57. [125] T. Link, F. Bellmann, H.M. Ludwig, M. Ben Haha, Reactivity and phase composition of Ca2SiO4 binders made by annealing of alpha-dicalcium silicate hydrate, Cement and Concrete Research, 67 (2015) 131-137. [126] S.N. Ghosh, P.B. Rao, A.K. Paul, K. Raina, The chemistry of dicalcium silicate mineral, Journal of Materials Science, 14 (1979) 1554-1566. [127] Y.J. Kim, I. Nettleship, W.M. Kriven, Phase Transformations in Dicalcium Silicate: II, TEM Studies of Crystallography, Microstructure, and Mechanisms, Journal of the American Ceramic Society, 75 (1992) 2407-2419. [128] H.-M. Ludwig, W. Zhang, Research review of cement clinker chemistry, Cement and Concrete Research, 78, Part A (2015) 24-37. [129] H. Ishida, S. Yamazaki, K. Sasaki, Y. Okada, T. Mitsuda, α-Dicalcium Silicate Hydrate: Preparation, Decomposed Phase, and Its Hydration, Journal of the American Ceramic Society, 76 (1993) 1707-1712. [130] K. Fukuda, N. Wakamatsu, S. Ito, Improvement in Hydration Reactivity of α-Phase Belite by Remelting Reaction, Journal of the American Ceramic Society, 84 (2001) 639-641. [131] K. Morsli, Á.G. De La Torre, S. Stöber, A.J.M. Cuberos, M. Zahir, M.A.G. Aranda, Quantitative Phase Analysis of Laboratory-Active Belite Clinkers by Synchrotron Powder Diffraction, Journal of the American Ceramic Society, 90 (2007) 3205-3212. [132] X. Li, W. Xu, S. Wang, M. Tang, X. Shen, Effect of SO3 and MgO on Portland cement clinker: Formation of clinker phases and alite polymorphism, Construction and Building Materials, 58 (2014) 182-192. [133] K. Fukuda, I. Maki, K. Toyoda, S. Ito, Kinetics of the α-to-α′H Polymorphic Phase Transition of Ca2SiO4 Solid Solutions, Journal of the American Ceramic Society, 76 (1993) 1821-1824. [134] I. Jelenić, A. Bezjak, M. Bujan, Hydration of B2O3-stabilized α′-and β-modifications of dicalcium silicate, Cement and Concrete Research, 8 (1978) 173-180. [135] Y.-M. Kim, S.-H. Hong, Influence of Minor Ions on the Stability and Hydration Rates of β-Dicalcium Silicate, Journal of the American Ceramic Society, 87 (2004) 900-905. [136] R. Trettin, G. Oliew, C. Stadelmann, W. Wieker, Very early hydration of dicalcium silicate-polymorphs, Cement and Concrete Research, 21 (1991) 757-764. [137] K. Fukuda, H. Taguchi, Hydration of α′L- and β-dicalcium silicates with identical concentration of phosphorus oxide, Cement and Concrete Research, 29 (1999) 503-506. [138] A.J.M. Cuberos, Á.G. De la Torre, M.C. Martín-Sedeño, L. Moreno-Real, M. Merlini, L.M. Ordónez, M.A.G. Aranda, Phase development in conventional and active belite cement pastes by Rietveld analysis and chemical constraints, Cement and Concrete Research, 39 (2009) 833-842. [139] L. Nicoleau, A. Nonat, D. Perrey, The di- and tricalcium silicate dissolutions, Cement and Concrete Research, 47 (2013) 14-30. [140] D. Damidot, F. Bellmann, B. Möser, T. Sovoidnich, Calculation of the dissolution rate of tricalcium silicate in several electrolyte compositions, Cement Wapno Beton, 12/74 (2007) 57-67. [141] P. Suraneni, M. Palacios, R.J. Flatt, New insights into the hydration of slag in alkaline media using a micro-reactor approach, Cement and Concrete Research, 79 (2016) 209-216. [142] F. Bellmann, D. Damidot, B. Möser, J. Skibsted, Improved evidence for the existence of an intermediate phase during hydration of tricalcium silicate, Cement and Concrete Research, 40 (2010) 875-884. [143] V. Kocaba, Development and evaluation of methods to follow microstructural development of cementitious systems including slags, in: Laboratoire des matériaux de construction, EPFL, 2009, pp. 145. [144] M.J. Whittaker, The Impact of Slag Composition on the Microstructure of Composite Slag Cements Exposed to Sulfate Attack, in: School of Civil Engineering University of Leeds, 2015, pp. 116. [145] A.C.A. Muller, K.L. Scrivener, A.M. Gajewicz, P.J. McDonald, Densification of C–S–H Measured by 1H NMR Relaxometry, The Journal of Physical Chemistry C, 117 (2013) 403-412. [146] W.A. Gutteridge, J.A. Dalziel, Filler cement: The effect of the secondary component on the hydration of Portland cement: Part I. A fine non-hydraulic filler, Cement and Concrete Research, 20 (1990) 778-782. [147] R.J. Flatt, G.W. Scherer, J.W. Bullard, Why alite stops hydrating below 80% relative humidity, Cement and Concrete Research, 41 (2011) 987-992. [148] F.A. Steele, W.P. Davey, THE CRYSTAL STRUCTURE OF TRICALCIUM ALUMINATE, Journal of the American Chemical Society, 51 (1929) 2283-2293. [149] P. Mondal, J.W. Jeffery, The crystal structure of tricalcium aluminate, Ca3Al2O6, Acta Cryst, B31 (1975) 689-697. [150] L. Gobbo, L.l. Sant'Agostino, L. Garcez, C3A polymorphs related to industrial clinker alkalies content, Cement and Concrete Research, 34 (2004) 657-664. [151] S.P. Varma, C.D. Wall, A monoclinic tricalcium aluminate (C3A) phase in a commercial Portland cement clinker, Cement and Concrete Research, 11 (1981) 567-574. [152] R.M. Herath Banda, F.P. Glasser, Crystallization of the molten phase in portland cement clinker, Cement and Concrete Research, 8 (1978) 665-670. [153] E. Breval, C3A hydration, Cement and Concrete Research, 6 (1976) 129-137. [154] L. Black, C. Breen, J. Yarwood, C.-S. Deng, J. Phipps, G. Maitland, Hydration of tricalcium aluminate (C3A) in the presence and absence of gypsum—studied by Raman spectroscopy and X-ray diffraction, Journal of Material Chemistry, 16 (2006) 1263 - 1272. [155] H.J. Kuzel, H. Pöllmann, Hydration of C3A in the presence of Ca(OH)2, CaSO4·2H2O and CaCO3, Cement and Concrete Research, 21 (1991) 885-895. [156] P. Meredith, A. Donald, N. Meller, C. Hall, Tricalcium aluminate hydration: Microstructural observations by in-situ electron microscopy, Journal of materials science, 39 (2004) 997-1005. [157] T.D. Ciach, E.G. Swenson, Morphology and microstructure of hydrating portland cement and its constituents I. Changes in hydration of tricalcium aluminate alone and in the presence of triethanolamine or calcium lignosulphonate, Cement and Concrete Research, 1 (1971) 143-158. [158] D. Stephan, S. Wistuba, Crystal structure refinement and hydration behaviour of doped tricalcium aluminate, Cement and Concrete Research, 36 (2006) 2011-2020. [159] M. Collepardi, G. Baldini, M. Pauri, M. Corradi, Tricalcium aluminate hydration in the presence of lime, gypsum or sodium sulfate, Cement and Concrete Research, 8 (1978) 571-580. [160] P. Hewlett, Lea's chemistry of cement and concrete, Butterworth-Heinemann, 2003. [161] H. Taylor, Cement chemistry, (1997). [162] J. Pourchez, P. Grosseau, B. Ruot, Current understanding of cellulose ethers impact on the hydration of C3A and C3A-sulphate systems, Cement and Concrete Research, 39 (2009) 664-669. [163] H. Minard, S. Garrault, L. Regnaud, A. Nonat, Mechanisms and parameters controlling the tricalcium aluminate reactivity in the presence of gypsum, Cement and Concrete Research, 37 (2007) 1418-1426. [164] L. Amathieu, T.A. Bier, K. Scrivener, Mechanisms of set acceleration of Portland cement through CAC addition, in: International conference on calcium aluminate cements, 2001, pp. 303-317. [165] P.K. Mehta, Effect of lime on hydration of pastes containing gypsum and calcium aluminates or calcium sulfoaluminate, Journal of the American Ceramic Society, 56 (1973) 315-319. [166] A.P. Kirchheim, V. Fernandez-Altable, P.J.M. Monteiro, D.C.C. Dal Molin, Analysis of cubic and orthorhombic C3A hydration in presence of gypsum and lime, Journal of Materials Science, 44 (2009) 2038 - 2045. [167] D.A. Silva, P.J. Monteiro, Early formation of ettringite in tricalcium aluminate–calcium hydroxide–gypsum dispersions, Journal of the American Ceramic Society, 90 (2007) 614-617. [168] J. Skalny, M. Tadros, Retardation of tricalcium aluminate hydration by sulfates, Journal of the American Ceramic Society, 60 (1977) 174-175. [169] M. Merlini, G. Artioli, T. Cerulli, F. Cella, A. Bravo, Tricalcium aluminate hydration in additivated systems. A crystallographic study by SR-XRPD, Cement and Concrete Research, 38 (2008) 477-486. [170] R.F. Feldman, V.S. Ramachandran, The influence of CaSO4.2H2O upon the hydration character of 3CaO.Al2O3, Magazine of Concrete Research, 18 (1966) 185 –196. [171] P. Gupta, S. Chatterji, J. Jeffery, Cement Technology 4, in, I-4, 1973. [172] H.J. Kuzel, Initial hydration reactions and mechanisms of delayed ettringite formation in Portland cements, Cement and Concrete Composites, 18 (1996) 195-203. [173] T. Matschei, B. Lothenbach, F.P. Glasser, The role of calcium carbonate in cement hydration, Cement and Concrete Research, 37 (2007) 551-558. [174] T. Matschei, B. Lothenbach, F.P. Glasser, The AFm phase in Portland cement, Cement and Concrete Research, 37 (2007) 118-130. [175] J.J. Beaudoin, V.S. Ramachandran, A new perspective on the hydration characteristics of cement phases, Cement and Concrete Research, 22 (1992) 689-694. [176] A. Quennoz, K.L. Scrivener, Hydration of C3A–gypsum systems, Cement and Concrete Research, 42 (2012) 1032-1041. [177] K. De Weerdt, K.O. Kjellsen, E. Sellevold, H. Justnes, Synergy between fly ash and limestone powder in ternary cements, Cement and Concrete Composites, 33 (2011) 30-38. [178] M. Zajac, A. Rossberg, G. Le Saout, B. Lothenbach, Influence of limestone and anhydrite on the hydration of Portland cements, Cement and Concrete Composites, 46 (2014) 99-108. [179] J.J. Beaudoin, V. Ramachandran, A new perspective on the hydration characteristics of cement phases, Cement and Concrete research, 22 (1992) 689-694. [180] C. Plowman, J. Cabrera, Mechanism and kinetics of hydration of C3A and C4AF. Extracted from cement, Cement and Concrete Research, 14 (1984) 238-248. [181] D.E. Rogers, L.P. Aldridge, Hydrates of calcium ferrites and calcium aluminoferrites, Cement and Concrete Research, 7 (1977) 399-409. [182] B.Z. Dilnesa, B. Lothenbach, G. Renaudin, A. Wichser, D. Kulik, Synthesis and characterization of hydrogarnet Ca3(AlxFe1 − x)2(SiO4)y(OH)4(3 − y), Cement and Concrete Research, 59 (2014) 96-111. [183] B.Z. Dilnesa, E. Wieland, B. Lothenbach, R. Dähn, K.L. Scrivener, Fe-containing phases in hydrated cements, Cement and Concrete Research, 58 (2014) 45-55. [184] B.Z. Dilnesa, B. Lothenbach, G. Renaudin, A. Wichser, E. Wieland, Stability of monosulfate in the presence of iron, Journal of the American Ceramic Society, 95 (2012) 3305-3316. [185] B.Z. Dilnesa, B. Lothenbach, G. Le Saout, G. Renaudin, A. Mesbah, Y. Filinchuk, A. Wichser, E. Wieland, Iron in carbonate containing AFm phases, Cement and Concrete Research, 41 (2011) 311-323. [186] G. Renaudin, A. Mesbah, B. Zeleke Dilnesa, M. Francois, B. Lothenbach, Crystal chemistry of iron containing cementitious AFm layered hydrates, Current Inorganic Chemistry, 5 (2015) 184-193. [187] B. EN197-1, Cement: composition, specifications and conformity criteria for common cements, British Standards Institution, London, (2011). [188] M. Öner, A study of intergrinding and separate grinding of blast furnace slag cement, Cement and Concrete Research, 30 (2000) 473-480. [189] H.M. Jennings, Colloid model of C−S−H and implications to the problem of creep and shrinkage Materials and Structures, 37 (2004) 59-70. [190] X. Wu, D.M. Roy, C.A. Langton, Early stage hydration of slag-cement, Cement and Concrete Research, 13 (1983) 277-286. [191] C. Çetin, S.T. Erdoğan, M. Tokyay, Effect of particle size and slag content on the early hydration of interground blended cements, Cement and Concrete Composites, 67 (2016) 39-49. [192] G. Puerta-Falla, A. Kumar, L. Gomez-Zamorano, M. Bauchy, N. Neithalath, G. Sant, The influence of filler type and surface area on the hydration rates of calcium aluminate cement, Construction and Building Materials, 96 (2015) 657-665. [193] K.L. Scrivener, A. Nonat, Hydration of cementitious materials, present and future, Cement and Concrete Research, 41 (2011) 651-665. [194] J. Duchesne, M.A. Be´rube´, Effect of supplementary cementing materials on the composition of cement hydration products, Advanced Cement Based Materials, 2 (1995) 43-52. [195] I.G. Richardson, A.R. Brough, G.W. Groves, C.M. Dobson, The characterization of hardened alkali-activated blast-furnace slag pastes and the nature of the calcium silicate hydrate (C-S-H) phase, Cement and Concrete Research, 24 (1994) 813-829. [196] J.I. Escalante-Garcia, J.H. Sharp, The chemical composition and microstructure of hydration products in blended cements, Cement and Concrete Composites, 26 (2004) 967-976. [197] M. Öner, K. Erdoğdu, A. Günlü, Effect of components fineness on strength of blast furnace slag cement, Cement and Concrete Research, 33 (2003) 463-469. [198] S. Kumar, R. Kumar, A. Bandopadhyay, T.C. Alex, B. Ravi Kumar, S.K. Das, S.P. Mehrotra, Mechanical activation of granulated blast furnace slag and its effect on the properties and structure of portland slag cement, Cement and Concrete Composites, 30 (2008) 679-685. [199] M.B. Haha, B. Lothenbach, G. Le Saout, F. Winnefeld, Influence of slag chemistry on the hydration of alkali-activated blast-furnace slag — Part II: Effect of Al2O3, Cement and Concrete Research, 42 (2012) 74-83. [200] I. Ismail, S.A. Bernal, J.L. Provis, R. San Nicolas, S. Hamdan, J.S.J. van Deventer, Modification of phase evolution in alkali-activated blast furnace slag by the incorporation of fly ash, Cement and Concrete Composites, 45 (2014) 125-135. [201] A. Schöler, B. Lothenbach, F. Winnefeld, M. Zajac, Hydration of quaternary Portland cement blends containing blast-furnace slag, siliceous fly ash and limestone powder, Cement and Concrete Composites, 55 (2015) 374-382. [202] M.B. Haha, B. Lothenbach, G. Le Saout, F. Winnefeld, Influence of slag chemistry on the hydration of alkali-activated blast-furnace slag — Part I: Effect of MgO, Cement and Concrete Research, 41 (2011) 955-963. [203] R. Snellings, Solution-controlled dissolution of supplementary cementitious material glasses at pH 13: The effect of solution composition on glass dissolution rates, J Am Ceram Soc, 96 (2013) 2467–2475. [204] C. Shi, R.L. Day, Some factors affecting early hydration of alkali-slag cements, Cement and Concrete Research, 26 (1996) 439-447. [205] J.I. Escalante-García, A.F. Fuentes, A. Gorokhovsky, P.E. Fraire-Luna, G. Mendoza-Suarez, Hydration Products and Reactivity of Blast-Furnace Slag Activated by Various Alkalis, Journal of the American Ceramic Society, 86 (2003) 2148-2153. [206] S.A. Bernal, R. San Nicolas, R.J. Myers, R. Mejía de Gutiérrez, F. Puertas, J.S.J. van Deventer, J.L. Provis, MgO content of slag controls phase evolution and structural changes induced by accelerated carbonation in alkali-activated binders, Cement and Concrete Research, 57 (2014) 33-43. [207] I.G. Richardson, J.G. Cabrera, The nature of CSH in model slag-cements, Cement and Concrete Composites, 22 (2000) 259-266. [208] N. Mobasher, S.A. Bernal, J.L. Provis, Structural evolution of an alkali sulfate activated slag cement, Journal of Nuclear Materials, 468 (2016) 97-104. [209] A.M. Rashad, Influence of different additives on the properties of sodium sulfate activated slag, Construction and Building Materials, 79 (2015) 379-389. [210] I.G. Richardson, Tobermorite/jennite- and tobermorite/calcium hydroxide-based models for the structure of C-S-H: applicability to hardened pastes of tricalcium silicate, β-dicalcium silicate, Portland cement, and blends of Portland cement with blast-furnace slag, metakaolin, or silica fume, Cement and Concrete Research, 34 (2004) 1733-1777. [211] I.G. Richardson, G.W. Groves, The structure of the calcium silicate hydrate phases present in hardened pastes of white Portland cement/blast-furnace slag blends, Journal of material Science, 32 (1997) 4793-4802. [212] E. Tajuelo Rodriguez, I.G. Richardson, L. Black, E. Boehm-Courjault, A. Nonat, J. Skibsted, Composition, silicate anion structure and morphology of calcium silicate hydrates (C-S-H) synthesised by silica-lime reaction and by controlled hydration of tricalcium silicate (C3S), Advances in Applied Ceramics, 114 (2015) 362-371. [213] M. Vandamme, F.-J. Ulm, P. Fonollosa, Nanogranular packing of C–S–H at substochiometric conditions, Cement and Concrete Research, 40 (2010) 14-26. [214] K. J. Krakowiak, W. Wilson, S. James, S. Musso, F.-J. Ulm, Inference of the phase-to-mechanical property link via coupled X-ray spectrometry and indentation analysis: Application to cement-based materials, Cement and Concrete Research, 67 (2015) 271-285. [215] S.P. Pandey, R.L. Sharma, The influence of mineral additives on the strength and porosity of OPC mortar, Cement and Concrete Research, 30 (2000) 19-23. [216] D.P. Bentz, Modeling the influence of limestone filler on cement hydration using CEMHYD3D, Cement and Concrete Composites, 28 (2006) 124-129. [217] I. Soroka, N. Stern, Calcareous fillers and the compressive strength of portland cement, Cement and Concrete Research, 6 (1976) 367-376. [218] I. Soroka, N. Setter, The effect of fillers on strength of cement mortars, Cement and Concrete Research, 7 (1977) 449-456. [219] V. Bonavetti, H. Donza, G. Menéndez, O. Cabrera, E.F. Irassar, Limestone filler cement in low w/c concrete: A rational use of energy, Cement and Concrete Research, 33 (2003) 865-871. [220] E.F. Irassar, D. Violini, V.F. Rahhal, C. Milanesi, M.A. Trezza, V.L. Bonavetti, Influence of limestone content, gypsum content and fineness on early age properties of Portland limestone cement produced by inter-grinding, Cement and Concrete Composites, 33 (2011) 192-200. [221] A.-M. Poppe, G. De Schutter, Cement hydration in the presence of high filler contents, Cement and Concrete Research, 35 (2005) 2290-2299. [222] M. Nehdi, S. Mindess, P.-C. Aïtcin, Optimization of high strength limestone filler cement mortars, Cement and Concrete Research, 26 (1996) 883-893. [223] T. Matschei, B. Lothenbach, F.P. Glasser, Thermodynamic properties of Portland cement hydrates in the system CaO–Al 2 O 3–SiO 2–CaSO 4–CaCO 3–H 2 O, Cement and Concrete Research, 37 (2007) 1379-1410. [224] G. Ye, X. Liu, G. De Schutter, A.M. Poppe, L. Taerwe, Influence of limestone powder used as filler in SCC on hydration and microstructure of cement pastes, Cement and Concrete Composites, 29 (2007) 94-102. [225] P. Mounanga, M.I.A. Khokhar, R. Hachem, A. Loukili, Improvement of the early-age reactivity of fly ash and blast furnace slag cementitious systems using limestone filler, Materials and Structures, 44 (2011) 437-453. [226] Y. Zhang, G. Ye, Effect of Limestone Powder on Microstructure of Ternary Cementitious System., Sustainable Construction Materials (2012) 225-234. [227] W.A. Klemm, L.D. Adams, An investigation of the formation of carboaluminates in: P. Klieger, R.D. Hooton (Eds.) Carbonate Additions to Cement, ASTM STP 1064, American Society for Testing and Materials, Philadelphia, 1990, pp. 60-72. [228] L. Basheer, J. Kropp, D.J. Cleland, Assessment of the durability of concrete from its permeation properties: a review, Construction and Building Materials, 15 (2001) 93-103. [229] P.H.R. Borges, J.O. Costa, N.B. Milestone, C.J. Lynsdale, R.E. Streatfield, Carbonation of CH and C–S–H in composite cement pastes containing high amounts of BFS, Cement and Concrete Research, 40 (2010) 284-292. [230] J.J. Chen, J.J. Thomas, H.M. Jennings, Decalcification shrinkage of cement paste, Cement and Concrete Research, 36 (2006) 801-809. [231] J. Kim, W.J. McCarter, B. Suryanto, S. Nanukuttan, P.A.M. Basheer, T.M. Chrisp, Chloride ingress into marine exposed concrete: A comparison of empirical- and physically- based models, Cement and Concrete Composites, 72 (2016) 133-145. [232] U. Balters, U. Ludwig, Influence of cement type on resistance against freezing and thawing, with or without deicing chemicals, of cement mortar, Frost Resistance of Concrete, 34 (2004) 119. [233] A. Marciniak, W. Grymin, T. Margiewicz, M. Koniorczyk, Influence of freezing-induced damage on the carbonation rate of concrete, European Journal of Environmental and Civil Engineering, (2016) 1-16. [234] J. Stark, A. Eckart, H.M. Ludwig, Influence of C3A content on frost and scaling resistance, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop on Resistance of Concrete to Freezing and Thawing With or Without De-icing Chemicals, E & FN SPON, University of Essen, 1997, pp. 100-109. [235] H. Toutanji, N. Delatte, S. Aggoun, R. Duval, A. Danson, Effect of supplementary cementitious materials on the compressive strength and durability of short-term cured concrete, Cement and Concrete Research, 34 (2004) 311-319. [236] G.J. Osborne, Durability of Portland blast-furnace slag cement concrete, Cement and Concrete Composites, 21 (1999) 11-21. [237] L.J. Parrott, Some effects of cement and curing upon carbonation and reinforcement corrosion in concrete, Materials and Structures, 29 (1996) 164-173 [238] O. Wowra, Effects of carbonation to microstructure and pore solution, in: N.J. Setzer, R. Auberg, I.J. Keck (Eds.) International RILEM Workshop on Frost Resistance of Concrete, 2002, pp. 61 - 68. [239] T. Grounds, H. Midgley, D. Novell, Carbonation of ettringite by atmospheric carbon dioxide, Thermochimica Acta, 135 (1988) 347-352. [240] E. Dubina, L. Korat, L. Black, J. Strupi-Šuput, J. Plank, Influence of water vapour and carbon dioxide on free lime during storage at 80 C, studied by Raman spectroscopy, Spectrochimica Acta Part A: Molecular and Biomolecular Spectroscopy, 111 (2013) 299-303. [241] L. Black, K. Garbev, I. Gee, Surface carbonation of synthetic CSH samples: A comparison between fresh and aged CSH using X-ray photoelectron spectroscopy, Cement and Concrete Research, 38 (2008) 745-750. [242] Z. Šauman, Effect of CO2 on porous concrete, Cement and Concrete Research, 2 (1972) 541-549. [243] E. Gruyaert, P. Van den Heede, N. De Belie, Carbonation of slag concrete: Effect of the cement replacement level and curing on the carbonation coefficient – Effect of carbonation on the pore structure, Cement and Concrete Composites, 35 (2013) 39-48. [244] E.T. Stepkowska, J.L. Pérez-Rodríguez, M.J. Sayagués, J.M. Martínez-Blanes, Calcite, vaterite and aragonite forming on cement hydration from liquid and gaseous phase, Journal of Thermal Analysis and Calorimetry 73 (2003) 247 - 269. [245] D. Russell, P.A.M. Basheer, G.I.B. Rankin, A.E. Long, Effect of relative humidity and air permeability on prediction of the rate of carbonation of concrete, Proceedings of the ICE - Structures and Buildings, 146 (2001) 319 - 326. [246] D.W.S. Ho, Q.Y. Cui, D.J. Ritchie, The influence of humidity and curing time on the quality of concrete, Cement and Concrete Research, 19 (1989) 457-464. [247] Z. Šauman, Carbonization of porous concrete and its main binding components, Cement and Concrete Research, 1 (1971) 645-662. [248] Z. Hu, M. Shao, Q. Cai, S. Ding, C. Zhong, X. Wei, Y. Deng, Synthesis of needle-like aragonite from limestone in the presence of magnesium chloride, Journal of Materials Processing Technology, 209 (2009) 1607-1611. [249] P. Pipilikaki, M. Beazi-Katsioti, The assessment of porosity and pore size distribution of limestone Portland cement pastes, Construction and Building Materials, 23 (2009) 1966-1970. [250] O. Çopuroğlu, A.L.A. Fraaij, J.M.J.M. Bijen, Effect of sodium monofluorophosphate treatment on microstructure and frost salt scaling durability of slag cement paste, Cement and Concrete Research, 36 (2006) 1475-1482. [251] B. Johannesson, P. Utgenannt, Microstructural changes caused by carbonation of cement mortar, Cement and Concrete Research, 31 (2001) 925-931. [252] G. Fagerlund, Internal frost attack - State of the art, in: M.J. Setzer, R. Auberg (Eds.) Frost Resistance of Concrete Proceedings of the International RILEM Workshop, Essen, 1997, pp. 321 - 338. [253] H.-J. Chen, S.-S. Huang, C.-W. Tang, M.A. Malek, L.-W. Ean, Effect of curing environments on strength, porosity and chloride ingress resistance of blast furnace slag cement concretes: A construction site study, Construction and Building Materials, 35 (2012) 1063-1070. [254] V.T. Ngala, C.L. Page, EFFECTS OF CARBONATION ON PORE STRUCTURE AND DIFFUSIONAL PROPERTIES OF HYDRATED CEMENT PASTES, Cement and Concrete Research, 27 (1997) 995-1007. [255] M. Pigeon, M. Setzer, ACTION OF FROST AND DEICING CHEMICALS-BASIC PHENOMENA AND TESTING, RILEM PROCEEDINGS 30 FREEZE-THAW DURABILITY OF CONCRETE, (1997). [256] J.J. Beaudoin, C. MacInnis, The mechanism of frost damage in hardened cement paste, Cement and Concrete Research, 4 (1974) 139-147. [257] M. Setzer, Action of frost and deicing chemicals: basic phenomena and testing, Freeze Thaw Durability of Concrete, (1976) 3-21. [258] O. Coussy, P.J.M. Monteiro, Poroelastic model for concrete exposed to freezing temperatures, Cement and Concrete Research, 38 (2008) 40-48. [259] O. Coussy, P. Monteiro, Unsaturated poroelasticity of freezing water-infiltrated materials with air voids, in: Poromechanics III-Biot Centennial (1905-2005): Proceedings of the 3rd Biot Conference on Poromechanics, 24-27 May 2005, Norman, Oklahoma, USA, CRC Press, 2005, pp. 457. [260] G.J. Verbeck, P. Klieger, Studies of'salt'scaling of concrete, Highway Research Board Bulletin, (1957). [261] O. Çopuroğlu, E. Schlangen, Modeling of frost salt scaling, Cement and Concrete Research, 38 (2008) 27-39. [262] V. Penttala, Surface and internal deterioration of concrete due to saline and non-saline freeze–thaw loads, Cement and Concrete Research, 36 (2006) 921-928. [263] J.S. Walder, B. Hallet, The physical basis of frost weathering: Toward a more fundamental and unified perspective, Artic and Alpine Research, 18 (1986) 27-32. [264] D.R. Uhlmann, B. Chalmers, K.A. Jackson, Interaction Between Particles and a Solid‐Liquid Interface, Journal of Applied Physics, 35 (1964) 2986-2993. [265] D.J. Janssen, The influence of material parameters on freeze-thaw resistance with and without deicing salt, in: M.J. Setzer, R. Auberg (Eds.) Proceedings of the Internal RILEM Workshop on Resistance of Concrete to Freezing and Thawing with or without De-icing Chemicals E&FN SPON, University of Essen, 1997, pp. 3-10. [266] A. Bilodeau, V.M. Malhotra, Deicing salt scaling resistance of concrete incorporating supplementary cementious materials: CANMET Research, in: J. Marchand, M. Pigeon, M. Setzer (Eds.) RILEM PROCEEDINGS 30 FREEZE-THAW DURABILITY OF CONCRETE, E and F Spon Limited, Quebec, Canada, 1997, pp. 121-156. [267] T.F. Rønning, Freeze-Thaw Resistance of Concrete: Effect of: Curing Conditions, Moisture Exchange and Materials, (2001). [268] W. Sun, Y.M. Zhang, H.D. Yan, R. Mu, Damage and damage resistance of high strength concrete under the action of load and freeze-thaw cycles, Cement and Concrete Research, 29 (1999) 1519-1523. [269] Z. Giergiczny, M.A. Glinicki, M. Sokołowski, M. Zielinski, Air void system and frost-salt scaling of concrete containing slag-blended cement, Construction and Building Materials, 23 (2009) 2451-2456. [270] C. Girodet, M. Chabannet, J. Bosc, J. Pera, Influence of the type of cement on the freeze-thaw resistance of the mortar phase of concrete, Frost Resistance of Concrete, 34 (2004) 34. [271] P. Taylor, Effect of Clinker Chemistry on Salt Scaling Resistance of Concrete, Transportation Research Record: Journal of the Transportation Research Board, 2113 (2009) 108-113. [272] H.F.W. Taylor, C. Famy, K.L. Scrivener, Delayed ettringite formation, Cement and Concrete Research, 31 (2001) 683-693. [273] A. Müller, C. Fuhr, D. Knöfel, Frost resistance of cement mortars with different lime contents, Cement and concrete research, 25 (1995) 809-818. [274] R. Bleszynski, R.D. Hooton, M.D. Thomas, C.A. Rogers, Durability of ternary blend concrete with silica fume and blast-furnace slag: laboratory and outdoor exposure site studies, ACI Materials Journal, 99 (2002) 499-508. [275] S.E. Chidiac, D.K. Panesar, Evolution of mechanical properties of concrete containing ground granulated blast furnace slag and effects on the scaling resistance test at 28days, Cement and Concrete Composites 30 (2008) 63-71 [276] M.S. Meddah, M.C. Lmbachiya, R.K. Dhir, Potential use of binary and composite limestone cements in concrete production, Construction and Building Materials, 58 (2014) 193-205. [277] B. Li, J. Wang, M. Zhou, Effect of limestone fines content in manufactured sand on durability of low- and high-strength concretes, Construction and Building Materials, 23 (2009) 2846-2850. [278] B. Espion, B. Lebon, C. Pierre, O. Germain, A. Hellebois, Characterisation of new ternary cements with reduced clinker content, in: Proceedings of the First International Conference on Concrete Sustainability, Japan Concrete Institute, 2013, pp. 145-152. [279] I.K. Battaglia, J.F. Munoz, S.M. Cramer, Proposed behavioral model for deicer scaling resistance of slag cement concrete, J Mater CivEng, 22 (2011) 361-368. [280] O. Çopuro, L. Fraaij, J. Bijen, Effect of curing conditions on freeze-thaw de-icing salt resistance of blast furnace slag cement mortars, WIT Transactions on The Built Environment, 76 (2004). [281] R.M. Geiker, Studies of Portland Cement Hydration: Measurements of Chemical Shrinkage and a Systematic Evaluaiton of Hydration Curves by Means of Dispersion Model, in: Technical University of Denmark, Technical University of Denmark, Technical University of Denmark, 1983. [282] J. Hjorth, J. Skibsted, H.J. Jakobsen, 29Si MAS NMR studies of portland cement components and effects of microsilica on the hydration reaction, Cement and Concrete Research, 18 (1988) 789-798. [283] A. Bentur, Effect of Gypsum on the Hydration and Strength of C3S Pastes, American Ceramic Society, 59 (1976) 210-213. [284] D. Ménétrier, I. Jawed, J. Skalny, Effect of gypsum on C3S hydration, Cement and Concrete Research, 10 (1980) 697-701. [285] I. Pane, W. Hansen, Investigation of blended cement hydration by isothermal calorimetry and thermal analysis, Cement and Concrete Research, 35 (2005) 1155-1164. [286] I. Wadsö, L. Wadsö, Systematic errors in isothermal micro-and nanocalorimetry, Journal of thermal analysis and calorimetry, 82 (2005) 553-558. [287] L. Wadsö, Operational issues in isothermal calorimetry, Cement and Concrete Research, 40 (2010) 1129-1137. [288] S.T. Bergold, F. Goetz-Neunhoeffer, J. Neubauer, Influence of the reactivity of the amorphous part of mechanically activated alite on its hydration kinetics, Cement and Concrete Research, 88 (2016) 73-81. [289] J.L. Poole, K.A. Riding, K.J. Folliard, M.C. Juenger, A.K. Schindler, Methods for calculating activation energy for Portland cement, ACI Materials Journal, 104 (2007) 86. [290] A. C1608-12, Standard Test Method for Chemical Shrinkage of Hydraulic Cement Paste, in, ASTM International, West Conshohocken, PA, 2012. [291] N. Setter, D.M. Roy, Mechanical features of chemical shrinkage of cement paste, Cement and Concrete Research, 8 (1978) 623-634. [292] T.C. Powers, T.L. Brownyard, Studies of the physical properties of hardened Portland cement paste, in: Journal Proceedings, 1946, pp. 101-132. [293] H.J.H. Brouwers, The work of Powers and Brownyard revisited: Part 1, Cement and Concrete Research, 34 (2004) 1697-1716. [294] M. Geiker, T. Knudsen, Chemical shrinkage of portland cement pastes, Cement and Concrete Research, 12 (1982) 603-610. [295] S. Boivin, P. Acker, S. Rigaud, B. Clavaud, Experimental assessment of chemical shrinkage of hydrating cement pastes, in: Autogenous shrinkage of concrete Spon Press, Proceedings of the International Workshop organized by the JCI (Japan Concrete Institute), 1999, pp. 81-92. [296] P. Lura, F. Winnefeld, S. Klemm, Simultaneous measurements of heat of hydration and chemical shrinkage on hardening cement pastes, Journal of Thermal Analysis and Calorimetry, 101 (2010) 925-932. [297] F. Lin, C. Meyer, Hydration kinetics modeling of Portland cement considering the effects of curing temperature and applied pressure, Cement and Concrete Research, 39 (2009) 255-265. [298] L.J. Parrott, M. Geiker, W.A. Gutteridge, D. Killoh, Monitoring Portland cement hydration: Comparison of methods, Cement and Concrete Research, 20 (1990) 919-926. [299] H.M. Dyson, I.G. Richardson, A.R. Brough, A Combined 29Si MAS NMR and Selective Dissolution Technique for the Quantitative Evaluation of Hydrated Blast Furnace Slag Cement Blends, J Am Ceram Soc, 90 (2007) 598-602. [300] L. McCusker, R. Von Dreele, D. Cox, D. Louer, P. Scardi, Rietveld refinement guidelines, Journal of Applied Crystallography, 32 (1999) 36-50. [301] G. Le Saoût, V. Kocaba, K. Scrivener, Application of the Rietveld method to the analysis of anhydrous cement, Cement and concrete research, 41 (2011) 133-148. [302] L. Mitchell, P. Whitfield, J. Beaudoin, The effects of particle statistics on quantitative Rietveld analysis of cement, in: 12th International congress on the Chemistry of Cement, Montreal, 2007, pp. 1-12. [303] R. Snellings, A. Bazzoni, K. Scrivener, The existence of amorphous phase in Portland cements: Physical factors affecting Rietveld quantitative phase analysis, Cement and Concrete Research, 59 (2014) 139-146. [304] W. Dollase, Correction of intensities for preferred orientation in powder diffractometry: application of the March model, Journal of Applied Crystallography, 19 (1986) 267-272. [305] N.C. Popa, Microstructural properties: Texture and macrostress effects, Chapter, 12 (2008) 332-375. [306] R. Von Dreele, Quantitative texture analysis by Rietveld refinement, Journal of Applied Crystallography, 30 (1997) 517-525. [307] D.L. Bish, S. Howard, Quantitative phase analysis using the Rietveld method, Journal of Applied Crystallography, 21 (1988) 86-91. [308] H. Rietveld, A profile refinement method for nuclear and magnetic structures, Journal of applied Crystallography, 2 (1969) 65-71. [309] K.L. Scrivener, T. Füllmann, E. Gallucci, G. Walenta, E. Bermejo, Quantitative study of Portland cement hydration by X-ray diffraction/Rietveld analysis and independent methods, Cement and Concrete Research, 34 (2004) 1541-1547. [310] D. Jansen, C. Stabler, F. Goetz-Neunhoeffer, S. Dittrich, J. Neubauer, Does Ordinary Portland Cement contain amorphous phase? A quantitative study using an external standard method, Powder Diffraction, 26 (2011) 31-38. [311] F.H. Chung, Quantitative interpretation of X-ray diffraction patterns of mixtures. I. Matrix-flushing method for quantitative multicomponent analysis, Journal of Applied Crystallography, 7 (1974) 519-525. [312] F.H. Chung, Quantitative interpretation of X-ray diffraction patterns of mixtures. III. Simultaneous determination of a set of reference intensities, Journal of Applied Crystallography, 8 (1975) 17-19. [313] D. Jansen, F. Goetz-Neunhoeffer, C. Stabler, J. Neubauer, A remastered external standard method applied to the quantification of early OPC hydration, Cement and Concrete Research, 41 (2011) 602-608. [314] P.M. Suherman, A. van Riessen, B. O’Connor, D. Li, D. Bolton, H. Fairhurst, Determination of amorphous phase levels in Portland cement clinker, Powder Diffraction, 17 (2002) 178-185. [315] G. Le Saout, K. Scrivener, Early Hydration of Portland Cement with Corundum Addition, in: 16 Internationale Baustofftagung (ibausil), Weimar, Germany, 2006, pp. 409-416. [316] A. De La Torre, S. Bruque, M. Aranda, Rietveld quantitative amorphous content analysis, Journal of Applied Crystallography, 34 (2001) 196-202. [317] I.C. Madsen, N.V. Scarlett, A. Kern, Description and survey of methodologies for the determination of amorphous content via X-ray powder diffraction, Zeitschrift für Kristallographie Crystalline Materials, 226 (2011) 944-955. [318] B.H. O'Connor, M.D. Raven, Application of the Rietveld refinement procedure in assaying powdered mixtures, Powder Diffraction, 3 (1988) 2-6. [319] C. Hesse, F. Goetz-Neunhoeffer, J. Neubauer, M. Braeu, P. Gaeberlein, Quantitative in situ X-ray diffraction analysis of early hydration of Portland cement at defined temperatures, Powder Diffraction, 24 (2009) 112-115. [320] S.T. Bergold, F. Goetz-Neunhoeffer, J. Neubauer, Quantitative analysis of C–S–H in hydrating alite pastes by in-situ XRD, Cement and Concrete Research, 53 (2013) 119-126. [321] N.C. Collier, J.H. Sharp, N.B. Milestone, J. Hill, I.H. Godfrey, The influence of water removal techniques on the composition and microstructure of hardened cement pastes, Cement and Concrete Research, 38 (2008) 737-744. [322] J. Zhang, G.W. Scherer, Comparison of methods for arresting hydration of cement, Cement and Concrete Research, 41 (2011) 1024-1036. [323] K.L. Scrivener, H. Patel, P. Pratt, L. Parrott, Analysis of phases in cement paste using backscattered electron images, methanol adsorption and thermogravimetric analysis, in: Mater Res Soc Symp Proc, Cambridge Univ Press, 1987, pp. 67-76. [324] P.J. Goodhew, J. Humphreys, R. Beanland, Electron microscopy and analysis, CRC Press, 2000. [325] H.S. Wong, M.K. Head, N.R. Buenfeld, Pore segmentation of cement-based materials from backscattered electron images, Cement and Concrete Research, 36 (2006) 1083-1090. [326] X. Feng, E.J. Garboczi, D.P. Bentz, P.E. Stutzman, T.O. Mason, Estimation of the degree of hydration of blended cement pastes by a scanning electron microscope point-counting procedure, Cement and Concrete Research, 34 (2004) 1787-1793. [327] T.C. Powers, Structure and physical properties of hardened Portland cement paste, Journal of the American Ceramic Society, 41 (1958) 1-6. [328] A.B. Abell, K.L. Willis, D.A. Lange, Mercury Intrusion Porosimetry and Image Analysis of Cement-Based Materials, Journal of Colloid and Interface Science, 211 (1999) 39-44. [329] S. Diamond, Mercury porosimetry: An inappropriate method for the measurement of pore size distributions in cement-based materials, Cement and Concrete Research, 30 (2000) 1517-1525. [330] P.J. McDonald, V. Rodin, A. Valori, Characterisation of intra- and inter-C–S–H gel pore water in white cement based on an analysis of NMR signal amplitudes as a function of water content, Cement and Concrete Research, 40 (2010) 1656-1663. [331] H. Elaqra, N. Godin, G. Peix, M. R'Mili, G. Fantozzi, Damage evolution analysis in mortar, during compressive loading using acoustic emission and X-ray tomography: Effects of the sand/cement ratio, Cement and Concrete Research, 37 (2007) 703-713. [332] E.W. Washburn, Note on a method of determining the distribution of pore sizes in a porous material, Proceedings of the National Academy of Sciences, 7 (1921) 115-116. [333] C. Gallé, Effect of drying on cement-based materials pore structure as identified by mercury intrusion porosimetry: A comparative study between oven-, vacuum-, and freeze-drying, Cement and Concrete Research, 31 (2001) 1467-1477. [334] L. Konecny, S. Naqvi, The effect of different drying techniques on the pore size distribution of blended cement mortars, Cement and concrete research, 23 (1993) 1223-1228. [335] H. Ma, Mercury intrusion porosimetry in concrete technology: tips in measurement, pore structure parameter acquisition and application, Journal of porous materials, 21 (2014) 207-215. [336] N. Hearn, R.D. Hooton, Sample mass and dimension effects on mercury intrusion porosimetry results, Cement and Concrete Research, 22 (1992) 970-980. [337] L. Tang, P.-E. Petersson, Slab test-freeze/Thaw resistance of concrete—Internal deterioration, Materials and Structures, 34 (2001) 526-531. [338] G.W. Scherer, Freezing gels, Journal of Non-Crystalline Solids, 155 (1993) 1-25. [339] B. Lothenbach, P. Durdzinski, K. De Weerdt, Chapter 5: Thermogravimetric Analysis, a practical guide to microstructural analysis of cementitious materials, Edt Karen Scrivener, Ruben Snellings, and Barbara Lothenbach, to be published byTaylor & Francis Group, (2016). [340] PDCEN/TR15177, Testing the freeze-thaw resistance of concrete-Internal structural damage, in, 2006. [341] E. Knapen, O. Cizer, K. Van Balen, D. Van Gemert, Effect of free water removal from early-age hydrated cement pastes on thermal analysis, Construction and Building Materials, 23 (2009) 3431-3438. [342] M. Whittaker, L. Black, Relationship between, early stage microstructure and long term durability of slag-containing cements, in: M. Russell (Ed.) 32nd Cement and Concrete Science Conference, Queens University Belfast, 2012, pp. 161-165. [343] L. Zhang, F. Glasser, Critical examination of drying damage to cement pastes, Advances in cement research, 12 (2000) 79-88. [344] R.L. Day, B.K. Marsh, Measurement of porosity in blended cement pastes, Cement and Concrete Research, 18 (1988) 63-73. [345] R.W. Cheary, A.A. Coelho, J.P. Cline, Fundamental parameters line profile fitting in laboratory diffractometers, J Res Natl Inst Stand Technol, 109 (2004) 1-25. [346] H. Morikawa, I. Minato, T. Tomita, S. Iwai, Anhydrite: a refinement, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 31 (1975) 2164-2165. [347] K. Ojima, Y. Nishihata, A. Sawada, Structure of potassium sulfate at temperatures from 296 K down to 15 K, Acta Crystallographica Section B: Structural Science, 51 (1995) 287-293. [348] H. Schmidt, I. Paschke, D. Freyer, W. Voigt, Water channel structure of bassanite at high air humidity: crystal structure of CaSO4· 0.625 H2O, Acta Crystallographica Section B: Structural Science, 67 (2011) 467-475. [349] W. Mumme, R. Hill, G. Bushnell-Wye, E. Segnit, Rietveld crystal structure refinements, crystal chemistry and calculated powder diffraction data for the polymorphs of dicalcium silicate and related phases, Neues Jahrbuch fur Mineralogie Abhandlungen, 169 (1995) 35-68. [350] A. Colville, S. Geller, The crystal structure of brownmillerite, Ca2FeAlO5, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 27 (1971) 2311-2315. [351] P. Mondal, J. Jeffery, The crystal structure of tricalcium aluminate, Ca3Al2O6, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 31 (1975) 689-697. [352] Y. Takeuchi, F. Nishi, Crystal-chemical characterization of the 3CaO· Al2O3—Na2O solid-solution series, Zeitschrift für Kristallographie-Crystalline Materials, 152 (1980) 259-308. [353] E. Maslen, V. Streltsov, N. Streltsova, N. Ishizawa, Electron density and optical anisotropy in rhombohedral carbonates. III. Synchrotron X-ray studies of CaCO3, MgCO3 and MnCO3, Acta Crystallographica Section B: Structural Science, 51 (1995) 929-939. [354] T. Pilati, F. Demartin, C. Gramaccioli, Lattice-dynamical estimation of atomic displacement parameters in carbonates: calcite and aragonite CaCO3, dolomite CaMg (CO3) 2 and magnesite MgCO3, Acta Crystallographica Section B: Structural Science, 54 (1998) 515-523. [355] G. Renaudin, R. Segni, D. Mentel, J.-M. Nedelec, F. Leroux, C. Taviot-Gueho, A Raman Study of the Sulfated Cement Hydrates: Ettringite and Monosulfoaluminate, Journal of Advanced Concrete Technology, 5 (2007) 299-312. [356] Á.G. De La Torre, S. Bruque, J. Campo, M.A. Aranda, The superstructure of C 3 S from synchrotron and neutron powder diffraction and its role in quantitative phase analyses, Cement and Concrete Research, 32 (2002) 1347-1356. [357] T. Runčevski, R.E. Dinnebier, O.V. Magdysyuk, H. Pöllmann, Crystal structures of calcium hemicarboaluminate and carbonated calcium hemicarboaluminate from synchrotron powder diffraction data, Acta Crystallographica Section B: Structural Science, 68 (2012) 493-500. [358] M. Bellotto, B. Rebours, O. Clause, J. Lynch, D. Bazin, E. Elkaïm, A reexamination of hydrotalcite crystal chemistry, The Journal of Physical Chemistry, 100 (1996) 8527-8534. [359] D. Taylor, Thermal expansion data. I: Binary oxides with the sodium chloride and wurtzite structures, MO, Transactions and journal of the British Ceramic Society, 83 (1984) 5-9. [360] D. Henderson, H. Gutowsky, A nuclear magnetic resonance determination of the hydrogen positions in Ca (OH) 2, in, DTIC Document, 1962. [361] Y. Le Page, G. Donnay, Refinement of the crystal structure of low-quartz, Acta Crystallographica Section B: Structural Crystallography and Crystal Chemistry, 32 (1976) 2456-2459. [362] D.C. Creagh, J.H. Hubbell, X-ray absorption (or attenuation) coefficients, International Tables for Crystallography, C (2006) 220-229. [363] V.S. Ramachandran, R.M. Paroli, J.J. Beaudoin, A.H. Delgado, Handbook of Thermal Analysis of Construction Materials, in, NOYES Publications, 2002, pp. 72-136. [364] R.S. Barneyback Jr, S. Diamond, Expression and analysis of pore fluids from hardened cement pastes and mortars, Cement and Concrete Research, 11 (1981) 279-285. [365] P.S. Whitfield, L.D. Mitchell, Quantitative Rietveld analysis of the amorphous content in cements and clinkers, Journal of Materials Science, 38 (2003) 4415-4421. [366] P. Scardi, Microstructural properties: lattice defects and domain size effects, Powder Diffraction Theory and Practice, (2008) 376-413. [367] Q. Zhou, F.P. Glasser, Thermal stability and decomposition mechanisms of ettringite at <120°C, Cement and Concrete Research, 31 (2001) 1333-1339. [368] J.H. Hubbell, Review and history of photon cross section calculationsWork supported by the National Institute of Standards and Technology, Physics in medicine and biology, 51 (2006) R245. [369] R. Snellings, —X-ray powder diffraction applied to cement, A Practical Guide to Microstructural Analysis of Cementitious Materials, (2016) 107. [370] A. Arora, G. Sant, N. Neithalath, Ternary blends containing slag and interground/blended limestone: Hydration, strength, and pore structure, Construction and Building Materials, 102, Part 1 (2016) 113-124. [371] I. Jawed, J. Skalny, Alkalies in cement: A review, Cement and Concrete Research, 8 (1978) 37-51. [372] L. Opoczky, Grinding technical questions of producing composite cements, Int J Miner Process, 44-45 (1996) 395-404. [373] A. Kumar, G. Sant, C. Patapy, C. Gianocca, K.L. Scrivener, The influence of sodium and potassium hydroxide on alite hydration: Experiments and simulations, Cement and Concrete Research, 42 (2012) 1513-1523. [374] T. Vuk, V. Tinta, R. Gabrovšek, V. Kaučič, The effects of limestone addition, clinker type and fineness on properties of Portland cement, Cement and Concrete Research, 31 (2001) 135-139. [375] K. Vance, M. Aguayo, T. Oey, G. Sant, N. Neithalath, Hydration and strength development in ternary portland cement blends containing limestone and fly ash or metakaolin, Cement and Concrete Composites, 39 (2013) 93-103. [376] A. Gruskovnjak, B. Lothenbach, F. Winnefeld, B. Münch, R. Figi, S.-C. Ko, M. Adler, U. Mäder, Quantification of hydration phases in supersulfated cements: review and new approaches, Adv Cem Res, 23 (2011) 265-275. [377] P.Z. Wang, R. Trettin, V. Rudert, Effect of fineness and particle size distribution of granulated blast-furnace slag on the hydraulic reactivity in cement systems, Advances in Cement Research, 17 (2005) 161-166. [378] J. J. Biernacki, J. M. Richardson, P. E. Stutzman, D.P. Bentz, Kinetics of Slag Hydration in the Presence of Calcium Hydroxide, J Am Ceram Soc, 85 (2002) 2261–2267. [379] S.C. Pal, A. Mukherjee, S.R. Pathak, Investigation of hydraulic activity of ground granulated blast furnace slag in concrete, Cement and Concrete Research, 33 (2003) 1481-1486. [380] H. Zhang, Z. Lin, D. Tong, Influence of the type of calcium sulfate on the strength and hydration of portland cement under an initial steam-curing condition, Cement and concrete research, 26 (1996) 1505-1511. [381] J. Cheung, A. Jeknavorian, L. Roberts, D. Silva, Impact of admixtures on the hydration kinetics of Portland cement, Cement and Concrete Research, 41 (2011) 1289-1309. [382] D. Rothstein, J.J. Thomas, B.J. Christensen, H.M. Jennings, Solubility behavior of Ca-, S-, Al-, and Si-bearing solid phases in Portland cement pore solutions as a function of hydration time, Cement and Concrete Research, 32 (2002) 1663-1671. [383] P. Monteiro, P.K. Mehta, Interaction between carbonate rock and cement paste, Cement and Concrete Research, 16 (1986) 127-134. [384] M.T. Palou, J. Majling, Effects of sulphate, calcium and aluminum ions upon the hydration of sulphoaluminate belite cement, Journal of thermal analysis, 46 (1996) 549-556. [385] D. Bentz, G. Sant, J. Weiss, Early-Age Properties of Cement-Based Materials. I: Influence of Cement Fineness, Journal of Materials in Civil Engineering 20 (2008) 502–508. [386] M. Collepardi, G. Baldini, M. Pauri, M. Corradi, The effect of pozzolanas on the tricalcium aluminate hydration, Cement and Concrete Research, 8 (1978) 741-751. [387] J. Péra, S. Husson, B. Guilhot, Influence of finely ground limestone on cement hydration, Cement and Concrete Composites, 21 (1999) 99-105. [388] T. Oey, A. Kumar, J.W. Bullard, N. Neithalath, G. Sant, The Filler Effect: The Influence of Filler Content and Surface Area on Cementitious Reaction Rates, J Am Ceram Soc, 96 (2013) 1978 - 1990. [389] E.H. Oelkers, General kinetic description of multioxide silicate mineral and glass dissolution, Geochimica et Cosmochimica Acta, 65 (2001) 3703-3719. [390] J.J. Thomas, H.M. Jennings, A colloidal interpretation of chemical aging of the C-S-H gel and its effects on the properties of cement paste, Cement and Concrete Research, 36 (2006) 30-38. [391] G.J. Stockmann, D. Wolff-Boenisch, N. Bovet, S.R. Gislason, E.H. Oelkers, The role of silicate surfaces on calcite precipitation kinetics, Geochimica et Cosmochimica Acta, 135 (2014) 231-250. [392] N. Voglis, G. Kakali, E. Chaniotakis, S. Tsivilis, Portland-limestone cements. Their properties and hydration compared to those of other composite cements, Cement and Concrete Composites, 27 (2005) 191-196. [393] M. Ben Haha, B. Lothenbach, G. Le Saout, F. Winnefeld, Influence of slag chemistry on the hydration of alkali-activated blast-furnace slag — Part I: Effect of MgO, Cement and Concrete Research, 41 (2011) 955-963. [394] O. Chowaniec, Limestone addition in cement., in: Laboratoire des matériaux de construction, EPFL, 2012. [395] L. Montanaro, A. Negro, M. Regourd, Action de CaCO3, CaSO4 et CaSO4· 2H2O sur l'Hydratation de C3S, Cement and Concrete Research, 18 (1988) 431-437. [396] A.P. Barker, An electron optical examination of zoning in blastfurnace slag hydrates: Part I. Slag cement pastes at early ages, Advances in Cement Research, 2 (1989) 171-179. [397] A. Vollpracht, B. Lothenbach, R. Snellings, J. Haufe, The pore solution of blended cements: a review, Materials and Structures, 49 (2016) 3341-3367. [398] D.-T. Nguyen, R. Alizadeh, J.J. Beaudoin, L. Raki, Microindentation creep of secondary hydrated cement phases and C–S–H, Materials and Structures, 46 (2013) 1519-1525. [399] EN206:2013, Concrete. Specification, performance, production and conformity, in, 2013. [400] C. Hall, Water sorptivity of mortars and concretes: a review, Magazine of Concrete Research, 41 (1989) 51-61. [401] M. Ghirci, S. Kenai, M. Said-Mansour, Mechanical properties and durability of mortar and concrete containing natural pozzolana and limestone blended cements, Cement and Concrete Composites, 29 (2007) 542-549. [402] V. Bonavetti, V. Rahhal, E.F. Irassar, Studies on the carboaluminate formation in limestone filler-blended cements, Cement and Concrete Research, 31 (2001) 853-859. [403] DDCEN/TS12390-9:2006, Testing hardened concrete. Freeze-thaw resistance. Scaling, in. [404] S. Rahman, Z. Grasley, E. Masad, D. Zollinger, S. Iyengar, R. Kogbara, Simulation of Mass, Linear Momentum, and Energy Transport in Concrete with Varying Moisture Content during Cooling to Cryogenic Temperatures, Transport in Porous Media, 112 (2016) 139-166. [405] H. Cai, X. Liu, Freeze-thaw durability of concrete: ice formation process in pores, Cement and Concrete Research, 28 (1998) 1281-1287. [406] T. RILEM, L.T. IDC, P. P-E, Final Recommendation of RILEM TC 176-IDC'Internal Damage of Concrete due to frost action', Materials and Structures, 37 (2004) 754-759. [407] P.A.M. Basheer, # Clam'permeability tests for assessing the durability of concrete, in, Queen's University of Belfast, 1991. [408] G. Fagerlund, The critical degree of saturation method of assessing the freeze/thaw resistance of concrete, Matériaux et Construction, 10 (1977) 217-229. [409] Z. Liu, W. Hansen, A hypothesis for salt frost scaling in cementitious materials, Journal of Advanced Concrete Technology, 13 (2015) 403-414. [410] Z. Liu, W. Hansen, Freezing characteristics of air-entrained concrete in the presence of deicing salt, Cement and Concrete Research, 74 (2015) 10-18. [411] S. Tsivilis, G. Batis, E. Chaniotakis, G. Grigoriadis, D. Theodossis, Properties and behavior of limestone cement concrete and mortar, Cement and Concrete Research, 30 (2000) 1679-1683. [412] A. Morandeau, M. Thiéry, P. Dangla, Impact of accelerated carbonation on OPC cement paste blended with fly ash, Cement and Concrete Research, 67 (2015) 226-236. [413] K. Suzuki, T. Nishikawa, S. Ito, Formation and carbonation of C-S-H in water, Cement and Concrete Research, 15 (1985) 213-224. [414] F. Sanchez, M.K. Langley White, A. Hoang, Leaching from granular cement-based materials during infiltration/wetting coupled with freezing and thawing, Journal of Environmental Management, 90 (2009) 983-993. [415] C. Carde, R. François, J.-M. Torrenti, Leaching of both calcium hydroxide and C-S-H from cement paste: Modeling the mechanical behavior, Cement and Concrete Research, 26 (1996) 1257-1268. [416] C. Gervais, A.C. Garrabrants, F. Sanchez, R. Barna, P. Moszkowicz, D.S. Kosson, The effects of carbonation and drying during intermittent leaching on the release of inorganic constituents from a cement-based matrix, Cement and Concrete Research, 34 (2004) 119-131. [417] T. Nishikawa, K. Suzuki, S. Ito, K. Sato, T. Takebe, Decomposition of synthesized ettringite by carbonation, Cement and Concrete Research, 22 (1992) 6-14. [418] A. Hidalgo, C. Domingo, C. Garcia, S. Petit, C. Andrade, C. Alonso, Microstructural changes induced in Portland cement-based materials due to natural and supercritical carbonation, Journal of Materials Science, 43 (2008) 3101-3111. [419] S.A. Bernal, M.C. Juenger, X. Ke, W. Matthes, B. Lothenbach, N. De Belie, J.L. Provis, Characterization of supplementary cementitious materials by thermal analysis, Materials and Structures, 50 (2017) 26. [420] L. Divet, R. Randriambololona, Delayed Ettringite Formation: The Effect of Temperature and Basicity on the Interaction of Sulphate and C-S-H Phase 1, Cement and Concrete Research, 28 (1998) 357-363. [421] J.J. Thomas, J.J. Chen, A.J. Allen, H.M. Jennings, Effects of decalcification on the microstructure and surface area of cement and tricalcium silicate pastes, Cement and Concrete Research, 34 (2004) 2297-2307. [422] J.E. Rossen, B. Lothenbach, K.L. Scrivener, Composition of C–S–H in pastes with increasing levels of silica fume addition, Cement and Concrete Research, 75 (2015) 14-22. [423] R.K. Iler, Effect of adsorbed alumina on the solubility of amorphous silica in water, Journal of Colloid and Interface Science, 43 (1973) 399-408. [424] L. Lam, Y.L. Wong, C.S. Poon, Degree of hydration and gel/space ratio of high-volume fly ash/cement systems, Cement and Concrete Research, 30 (2000) 747-756."],"dcterms:accessrights":["public"],"dc:title":["Relationship between Microstructure, Durability and Performance of CEM X Composite Cements"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"]},"updated_at":"2026-11-18T22:21:38Z"}