{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:27926"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:27926","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"An Assessment of the Effect of Machining and Forging Texture on the Fatigue Performance of Aerospace Titanium Alloys","abstract":"Safety-critical aerospace jet engine components such as titanium alloy compressor discs are manufactured under very strict standards and regulations. It is essential that the effects of every manufacturing stage is fully understood to ensure the best performance and avoid catastrophic failures. In this study the effects of upstream forging and downstream machining were determined and correlated with the variable fatigue performance of a number of Rolls-Royce Ti-6Al-2Sn-4Zr-6Mo compressor disc forgings used in the intermediate pressure section of a gas turbine aero-engine. A four-point flexural testing approach was used to characterise the fatigue life heterogeneity at different circumferential locations in a Ti-6Al-2Sn-4Zr-6Mo compressor discs. Texture analysis using electron backscattered diffraction linked these fatigue life differences with the heterogeneous nonlinear strain pattern induced during the open die hot forging process at the primary forging stage of the VAR ingot. Moreover, this texture analysis also revealed the alignment of the HCP crystal c-axis in the radial direction parallel to the hoop stress during the close die forging secondary forging. Crack initiation analysis of fatigue test coupons of these regions were dominated with alpha phase that was orientated at an angle of 20-40o with respect to the loading direction. This demonstrated that there is no purely basal cleavage and a component of the applied stress has been transformed into deformation slip to initiate a crack. EBSD analysis was performed to understand the crack propagation mechanisms after identifying different crack path geometries during fractography analysis. Best performing circumferential regions displayed a more convoluted crack path and a lower texture index (MUD), as opposed to the straight cracks in the worst performing regions. This was directly correlated to the texture heterogeneities induced during forging. Moreover, the best performing samples showed crack diversion/arrest when the crack tip encountered regions unfavourably orientated for prismatic slip with respect to the loading direction. A small-scale machining test was developed to recreate the industrial face turning process in small samples, making it more resource efficient to test different machining parameters. This process was used to machine flat coupons, extracted from a second Ti-6Al-2Sn-4Zr-6Mo alloy forged disc, which were subsequently tested in the 4-point bend fatigue approach. This enabled the effects of machining parameters on the surface performance to be directly correlated to the fatigue life. Results showed that faster cutting speeds and metal removal rates did not have any detrimental effect on fatigue life. In fact, machined coupons presented up to three times the fatigue life compared to non-machined ones. However, circumferential variation in fatigue life was still present, suggesting that the inherent forging effects on fatigue life cannot be “erased” through the machining process. A third Ti-6Al-2Sn-4Zr-6Mo disc was machined at Rolls- Royce facilities to evaluate the capabilities of the production machines when machining at higher speeds. Vibrations in the component and mid-range speeds induced chattering which produced distinct surface markings. However, this effect was not seen at the current industry standard or fastest machining speeds. This was attributed to modal frequencies and system vibrations. Finally, force feedback analysis (FFA) has been used to characterise the microstructure of a range of titanium alloys (and heat treatment conditions) through the measured cutting forces. Heterogeneous cutting performance has been linked to the primary forging process, demonstrated in a Ti-54M forged billet, and a closer inspection of the collected signal, allowed grain size measurements and microstructural features reconstruction in ”fingerprint diagrams”. This reconstruction was validated using in a �-forged Ti-17 billet.","abstract_html":"Safety-critical aerospace jet engine components such as titanium alloy compressor discs are manufactured under very strict standards and regulations. It is essential that the effects of every manufacturing stage is fully understood to ensure the best performance and avoid catastrophic failures. In this study the effects of upstream forging and downstream machining were determined and correlated with the variable fatigue performance of a number of Rolls-Royce Ti-6Al-2Sn-4Zr-6Mo compressor disc forgings used in the intermediate pressure section of a gas turbine aero-engine. A four-point flexural testing approach was used to characterise the fatigue life heterogeneity at different circumferential locations in a Ti-6Al-2Sn-4Zr-6Mo compressor discs. Texture analysis using electron backscattered diffraction linked these fatigue life differences with the heterogeneous nonlinear strain pattern induced during the open die hot forging process at the primary forging stage of the VAR ingot. Moreover, this texture analysis also revealed the alignment of the HCP crystal c-axis in the radial direction parallel to the hoop stress during the close die forging secondary forging. Crack initiation analysis of fatigue test coupons of these regions were dominated with alpha phase that was orientated at an angle of 20-40o with respect to the loading direction. This demonstrated that there is no purely basal cleavage and a component of the applied stress has been transformed into deformation slip to initiate a crack. EBSD analysis was performed to understand the crack propagation mechanisms after identifying different crack path geometries during fractography analysis. Best performing circumferential regions displayed a more convoluted crack path and a lower texture index (MUD), as opposed to the straight cracks in the worst performing regions. This was directly correlated to the texture heterogeneities induced during forging. Moreover, the best performing samples showed crack diversion/arrest when the crack tip encountered regions unfavourably orientated for prismatic slip with respect to the loading direction. A small-scale machining test was developed to recreate the industrial face turning process in small samples, making it more resource efficient to test different machining parameters. This process was used to machine flat coupons, extracted from a second Ti-6Al-2Sn-4Zr-6Mo alloy forged disc, which were subsequently tested in the 4-point bend fatigue approach. This enabled the effects of machining parameters on the surface performance to be directly correlated to the fatigue life. Results showed that faster cutting speeds and metal removal rates did not have any detrimental effect on fatigue life. In fact, machined coupons presented up to three times the fatigue life compared to non-machined ones. However, circumferential variation in fatigue life was still present, suggesting that the inherent forging effects on fatigue life cannot be “erased” through the machining process. A third Ti-6Al-2Sn-4Zr-6Mo disc was machined at Rolls- Royce facilities to evaluate the capabilities of the production machines when machining at higher speeds. Vibrations in the component and mid-range speeds induced chattering which produced distinct surface markings. However, this effect was not seen at the current industry standard or fastest machining speeds. This was attributed to modal frequencies and system vibrations. Finally, force feedback analysis (FFA) has been used to characterise the microstructure of a range of titanium alloys (and heat treatment conditions) through the measured cutting forces. Heterogeneous cutting performance has been linked to the primary forging process, demonstrated in a Ti-54M forged billet, and a closer inspection of the collected signal, allowed grain size measurements and microstructural features reconstruction in ”fingerprint diagrams”. This reconstruction was validated using in a �-forged Ti-17 billet.","abstract_has_math":false,"creators":["Suárez Fernández, Daniel"],"institution":"University of Sheffield","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Jackson, Martin","Wynne, Bradley","Fox, Kate"],"committee_chairs":[],"committee_members":[],"year":2020,"date_issued":"2020-04","date_published":"2020-04","updated_at":"2026-11-18T22:40:18Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.816932"],"render_values":[{"text":"uk.bl.ethos.816932","href":null,"code":true}]},{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["EP/L016273"],"render_values":[{"text":"EP/L016273","href":null,"code":true}]}],"person_identifier_entries":[{"key":"person:identifier.orcid","label":"ORCID","values":["0000000151998761"],"render_values":[{"text":"0000-0001-5199-8761","href":"https://orcid.org/0000-0001-5199-8761","code":true}]}]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/27926/1/CR.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A27926","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Jackson, Martin","Wynne, Bradley","Fox, Kate"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["EPSRC"]},{"key":"dc:creator","label":"Author","values":["Suárez Fernández, Daniel"]},{"key":"person:identifier.orcid","label":"ORCID","values":["0000000151998761"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2020-04"]},{"key":"dc:date.issued","label":"Date","values":["2020-04"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Materials Science and Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/27926/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["[1] Roskill Market Reports and Consultancy, “Titanium Metal: Global Industry, Markets & Outlook,” tech. rep., Roskill, 2018. [2] N. Lecca, “Airbus commercial aircraft results 2017,” tech. rep., Airbus, 2018. [3] Airbus S.A.S. (Airbus Group), “Taking the lead: The A350XWB,” 2006. [4] J. Halford, “Driving Growth through Innovation Commercial and Military Titanium Demand Trends,” tech. rep., Arconic, Singapore, 2018. [5] E. Schulz, “Global Market Forecast: Growing Horizons 2017/2036,” Airbus Global Market Forecast, 2018. [6] N. Tian, A. Fleurant, A. Kuimova, P. Wezeman, and S. Wezeman, “Trends in World Military Expenditure, 2017,” Tech. Rep. May, Stockholm International Peace Research Institute, Stockholm, 2018. [7] S. Seong, O. Younossi, and B. W. Goldsmith, “Titanium Industrial Base, Price Trends, and Technology Initiatives,” tech. rep., RAND, 2009. [8] European Comission, “Climate Action: Reducing emissions from aviation.” [9] European Parliament, “Regulation (EU) No 598/2014 of the European Parliament and of the Council of 16 April 2014 on the establishment of rules and procedures with regard to the introduction of noise-related operating restrictions at Union airports within a Balanced Approach,” Tech. Rep. 598, European Union, 2014. [10] European Comission, “Aircraft Noise.” [11] Aviation Safety Network (Flight Safety Foundation), “Number of airliner accidents per,” 2018. [12] National Transportation Safety Board, “In Reply refer to: A-90-167 National Transportation Safety Board,” tech. rep., National Transportation Safety Board, 1990. [13] National Transportation Safety Board, “Aircraft Accident Report: United Airlines Flight 232, McDonnell Douglas DC-I0-10, Sioux Gateway Airport, Sioux City, Iowa, July 19 1989,” tech. rep., National Transportation Safety Board, 1989. [14] M. C. Blakey, “Safety Recommendation: In reply refer to: A-06-60 through -64,” tech. rep., National Transportation Safety Board, 2006. [15] National Transportation Safety Board, “Uncontained Engine Failure and Subsequent Fire, American Airlines Flight 383, Boeing 767-323, N345AN, Chicago, Illinois, October 28, 2016,” tech. rep., National Transportation Safety Board, 2016. [16] Australian Transport Safety Bureau, “In-flight uncontained engine failure A380- 842, VH-OQA,” Tech. Rep. June, Australian Transport Safety Bureau, 2013. [17] R.-R. plc, “Annual Report 2017 Rolls-Royce Holdings plc,” tech. rep., Rolls-Royce Holdings plc, 2017. [18] J. Esslinger, “Titanium in Aero Engines Demands on Titanium Alloys and Processes in Aero Engines,” Proceedings of the 10thWorld Conference on Titanium (Ti-2003), pp. 2845–2852, 2003. [19] N. S. Weston and M. Jackson, “FAST-forge − A new cost-effective hybrid processing route for consolidating titanium powder into near net shape forged components,” Journal of Materials Processing Technology, vol. 243, pp. 335–346, 2017. [20] F. Martina and S. Williams, “Wire+arc additive manufacturing vs. traditional machining from solid: a cost comparison,” tech. rep., Cranfield University, 2015. [21] B. Hurles and F. Froes, “Lowering the cost of titanium,” AMPTIAC Quarterly, vol. 6, no. 2, 2002. [22] P. Mallick, C. Horvath, J. Benedyk, B. Powell, A. Luo, P. Krajewski, G. T. Kridli, P. A. Friedman, J. M. Boileau, S. Das, and A. Deb, Materials, Design and Manufacturing for Lightweight Vehicles. CRC, 2010. [23] F. H. Froes, H. Friedrich, J. Kiese, and D. Bergoint, “Titanium in the family automobile: The cost challenge,” Cost - Affordable Titanium, Symposium, dedicated to Professor Harvey Flower, no. February 2004, pp. 159–166, 2004. [24] A. Acharya and V. A. Gokhale, “Titanium: A New Generation Material for Architectural Applications,” International Journal of Engineering Research and Applications, vol. 05, no. 02, pp. 22–29, 2015. [25] G. Lutjering and J. Williams, Engineering Materials and Processes: Titanium. Springer, 2007. [26] M. George and USGS (United States Geological Survey), “Titanium and Titanium Dioxide (USGS),” tech. rep., United States Geological Survey, 2020. [27] A. Zarkades and F. Larson, “Elasticity of Titanium Sheet Alloys,” in The Science, Technology and Application of Titanium, pp. 933–941, Pergamon Press Ltd, 1970. [28] G. Lütjering and J. C. Williams, Titanium Book. Springer, 2007. [29] M. J. Donachie, Titanium - A Technical Guide. ASM International, 2000. [30] R. R. Boyer, “Aerospace applications of beta titanium alloys,” Jom, vol. 46, no. 7, pp. 20–23, 1994. [31] TIMET Ltd., “Timetal 6-2-4-6 Mechanical Properties,” 2019. [32] T. Krull, J. Albrecht, and G. Lüetjering, “The Effect of Yield Stress Level on the Mechanical Properties of Ti-6246,” Science and Technology, The Japan Institute of Metals, pp. 519–522, 2007. [33] S. Kathleen, S. Dragolich, N. D. DiMatteo, and S. D. Henry, Fatigue Data Book: Light Structural Alloys. ASM (American Society of Metals), 1994. [34] C. E. W. Boyer R., Welsch G., Materials Properties Handbook: Titanium Alloys. ASM International, 1994. [35] SAE Aerospace, “Aerospace Material Specification SAE AMS 4981E, Titanium Alloy Bars, Wire, and Forgings 6.0Al - 2.0Sn - 4.0Zr - 6.0Mo Solution and Precipitation Heat Treated,” 2006. [36] D. R. N. Correa, F. B. Vicente, R. O. Araújo, M. L. Lourenço, P. A. B. Kuroda, M. A. R. Buzalaf, and C. R. Grandini, “Effect of the substitutional elements on the microstructure of the Ti-15Mo-Zr and Ti-15Zr-Mo systems alloys,” Journal of Materials Research and Technology, vol. 4, no. 2, pp. 180–185, 2015. [37] A. Banerjee, S. Balachandran, S. Suwas, and D. Banerjee, “Deformation Behaviour of Titanium Alloys Ti-6242 and Ti-6246,” Proceedings of the 13th World Conference on Titanium, no. Table I, pp. 1095–1101, 2016. [38] R. Wanhill and S. Barter, Fatigue of Beta Processed and Beta Heat-treated Titanium Alloys. Springer Science and Business Media, 2011. [39] S. Hémery and P. Villechaise, “Comparison of slip system activation in Ti-6Al-2Sn- 4Zr-2Mo and Ti-6Al-2Sn-4Zr-6Mo under tensile, fatigue and dwell-fatigue loadings,” Materials Science and Engineering A, vol. 697, no. March, pp. 177–183, 2017. [40] I. Inagaki, T. Takechi, S. Yoshihisa, and A. Nozomu, “Application and Features of Titanium for the Aerospace Industry,” Nippon Steel & Sumitomo Metal Technical Report, no. 106, pp. 22–27, 2014. [41] D. Eylon, S. Fujishiro, and F. H. Froes, “Titanium Alloys for High Temperature Applications — a Review,” High Temperature Materials and Processes, vol. 6, no. 1- 2, pp. 81–92, 1984. [42] M. Evans and A. R. Ward, “Corrosion resistance of Ti-6246 for high power aeroengine compressor discs and blades,” Materials Science and Technology, vol. 17, no. 8, pp. 945–953, 2001. [43] S. Joseph, T. C. Lindley, D. Dye, and E. A. Saunders, “The mechanisms of hot salt stress corrosion cracking in titanium alloy Ti-6Al-2Sn-4Zr-6Mo,” Corrosion Science, vol. 134, pp. 169–178, 2018. [44] D. Banerjee and J. C. Williams, “Perspectives on titanium science and technology,” Acta Materialia, vol. 61, no. 3, pp. 844–879, 2013. [45] Z. Zheng, D. S. Balint, and F. P. E. Dunne, “Dwell fatigue in two Ti alloys: An integrated crystal plasticity and discrete dislocation study,” Journal of the Mechanics and Physics of Solids, vol. 96, pp. 411–427, 2016. [46] M. R. Bache, M. Cope, H. M. Davies, W. J. Evans, and G. Harrison, “Dwell sensitive fatigue in a near alpha titanium alloy at ambient temperature,” International Journal of Fatigue, vol. 19, no. SUPPL.1, pp. 83–88, 1997. [47] J. Qiu, Y. Ma, J. Lei, Y. Liu, A. Huang, D. Rugg, and R. Yang, “A Comparative Study on Dwell Fatigue of Ti-6Al-2Sn-4Zr-xMo (x = 2 to 6) Alloys on a Microstructure-Normalized Basis,” Metallurgical and Materials Transactions A: Physical Metallurgy and Materials Science, vol. 45, no. 13, pp. 6075–6087, 2014. [48] R. B. Osman and M. V. Swain, “A critical review of dental implant materials with an emphasis on titanium versus zirconia,” Materials, vol. 8, no. 3, pp. 932–958, 2015. [49] C. Leyens and M. Peters, Titanium and Titanium Alloys. Wiley-VCH, 2003. [50] D. Williams, “The effects of zirconium in titanium-base alloys,” Journal of less common metals, vol. 6, pp. 219–225, 1964. [51] D. R. N. Correa, F. B. Vicente, T. A. G. Donato, V. E. Arana-Chavez, M. A. R. Buzalaf, and C. R. Grandini, “The effect of the solute on the structure, selected mechanical properties, and biocompatibility of Ti-Zr system alloys for dental applications,” Materials Science and Engineering C, vol. 34, no. 1, pp. 354–359, 2014. [52] W. G. Burgers, “W.G. Burgers Physica 1934.pdf,” Physica, vol. 1, no. 7-12, pp. 549– 560, 1933. [53] V. Tong, S. Joseph, A. K. Ackerman, D. Dye, and T. B. Britton, “Using transmission Kikuchi diffraction to characterise alpha variants in an alpha + beta titanium alloy,” Journal of Microscopy, vol. 267, no. 3, pp. 318–329, 2016. [54] T. B. Britton, J. Jiang, Y. Guo, A. Vilalta-Clemente, D. Wallis, L. N. Hansen, A. Winkelmann, and A. J. Wilkinson, “Tutorial: Crystal orientations and EBSD - Or which way is up?,” Materials Characterization, vol. 117, pp. 113–126, 2016. [55] M. G. Glavicic, B. B. Bartha, S. K. Jha, and C. J. Szczepanski, “The origins of microtexture in duplex Ti alloys,” Materials Science and Engineering A, vol. 513- 514, no. C, pp. 325–328, 2009. [56] E. Lee, R. Banerjee, S. Kar, D. Bhattacharyya, and H. L. Fraser, “Selection of � variants during microstructural evolution in �/� titanium alloys,” Philosophical Magazine, vol. 87, no. 24, pp. 3615–3627, 2007. [57] J. Walter, M. Jackson, and C. Sims, Titanium and its alloys: Principles of Alloying Titanium. ASM International, 1988. [58] G. Lütjering, “Influence of processing on microstructure and mechanical properties of (� + �) titanium alloys,” Materials Science and Engineering A, vol. 243, no. 1-2, pp. 32–45, 1998. [59] J. B. Borradaile and R. H. Heal, “Critical Review Mechanical Properties of Titanium Alloys,” Proc. Titanium, vol. 1, pp. 141–152, 1980. [60] T. Choda, H. Oyama, and S. Murakami, “Technology for process design of titanium alloy forging,” Journal of Japan Institute of Light Metals, vol. 65, no. 9, pp. 460–465, 2015. [61] Z. Z. Fang, J. D. Paramore, P. Sun, K. S. Chandran, Y. Zhang, Y. Xia, F. Cao, M. Koopman, and M. Free, “Powder metallurgy of titanium–past, present, and future,” International Materials Reviews, vol. 63, no. 7, pp. 407–459, 2018. [62] C. Brooks, Heat treatment, structure and properties of nonferrous alloys. ASM (American Society of Metals), 1982. [63] J. Xu, Z. Zhang, P. Fang, and W. Hu, “Summary Abstract: Comparison of ingot structure of vacuum arc remelting–vacuum arc double‐electrode remelting processes: Study of the possibility of using cast titanium directly as an isothermo‐forging billet,” Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films, vol. 5, no. 4, pp. 2682–2683, 1987. [64] R. C. Atwood, P. D. Lee, R. S. Minisandram, and R. M. Jones, “Multiscale modelling of microstructure formation during vacuum arc remelting of titanium 6-4,” Journal of Materials Science, vol. 39, no. 24, pp. 7193–7197, 2004. [65] I. Weiss and S. L. Semiatin, “Thermomechanical processing of alpha titanium alloys - An overview,” Materials Science and Engineering A, vol. 263, no. 2, pp. 243–256, 1999. [66] J. D. Cotton, R. D. Briggs, R. R. Boyer, S. Tamirisakandala, P. Russo, N. Shchetnikov, and J. C. Fanning, “State of the Art in Beta Titanium Alloys for Airframe Applications,” Jom, vol. 67, no. 6, pp. 1281–1303, 2015. [67] Z. Guo and T. Baker, “On the microstructure and thermomechanical processing of titanium alloy IMI685,” Materials Science and Engineering A, vol. 1, no. 1, pp. 63–76, 1992. [68] P. Davies, An Investigation of Microstructure and Texture Evolution in the Near-� Titanium Alloy Timetal 834. PhD thesis, The University of Sheffield, 2009. [69] P. Partridge, “The crystallography and deformation modes of hexagonal closepacked metals,” Metallurgical Reviews, vol. 6690, pp. 169–194, 1967. [70] M. H. Yoo, “Slip, twinning, and fracture in hexagonal close-packed metals,” Metallurgical Transactions A, vol. 12, no. 3, pp. 409–418, 1981. [71] D. G. R. William D. Callister, Jr., Materials Science and Engineering An introduction, vol. 1. John Wiley & Sons, 8th ed., 2010. [72] S. L. Semiatin, T. R. Bieler, and I. Introduction, “Effect of Texture and Slip Mode on the Anisotropy of Plastic Flow and Flow Softening during Hot Working of Ti- 6Al-4V,” Metallurgical and Materials Transactions A: Physical Metallurgy and Materials Science, vol. 32, no. July, 2001. [73] Y. C. Lin, B. H. Yan, and Y. S. Chang, “Machining characteristics of titanium alloy (Ti-6Al-4V) using a combination process of EDM with USM,” Journal of Materials Processing Technology, vol. 104, no. 3, pp. 171–177, 2000. [74] S. Kuriakose and M. S. Shunmugam, “Characteristics of wire-electro discharge machined Ti6Al4V surface,” Materials Letters, vol. 58, no. 17-18, pp. 2231–2237, 2004. [75] T. Ahmed and H. J. Rack, “Phase transformations during cooling in alpha + beta titanium alloys,” 1998. [76] A. Hasçalik and U. Çaydaş, “Electrical discharge machining of titanium alloy (Ti- 6Al-4V),” Applied Surface Science, vol. 253, no. 22, pp. 9007–9016, 2007. [77] F. Klocke, D. Welling, and J. Dieckmann, “Comparison of grinding and Wire EDM concerning fatigue strength and surface integrity of machined Ti6Al4V components,” Procedia Engineering, vol. 19, no. December 2011, pp. 184–189, 2011. [78] M. Manjaiah, S. Narendranath, and S. Basavarajappa, “A Reviwe on Machining of Titanium Based Alloys Using EDM and WEDM,” Reviews on advanced materials science, vol. 36, pp. 89–111, 2014. [79] ASTM, “Standard Test Method for Strain-Controlled Fatigue Testing,” Tech. Rep. 2004, ASTM, 2004. [80] ASTM, “Astm E399,” tech. rep., ASTM, 2016. [81] ASTM, “ASTM D790-03.Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials.American Society for Testing and Materials. United States of America,” tech. rep., ASTM, 2017. [82] A. Cox, Understanding the effect of surface generation rates for finish milling of aero-structural components. PhD thesis, The University of Sheffield, 2017. [83] A. Cox, S. Herbert, J. P. Villain-Chastre, S. Turner, and M. Jackson, “The effect of machining and induced surface deformation on the fatigue performance of a high strength metastable � titanium alloy,” International Journal of Fatigue, vol. 124, no. February, pp. 26–33, 2019. [84] M. Whittaker, Titanium in the Gas Turbine Engine. INTECH, 2011. [85] D. Tromans, “Elastic Anisotropy of HCP Metal Crystals and Polycrystals,” Ijrras, vol. 6, no. March, pp. 462–483, 2011. [86] R. Weaver, “Rediscovering Polarized Light Microscopy,” Tech. Rep. October, AMERICAN LABORATORY, 2003. [87] R. Oldenbourg, “A new view on polarization microscopy.,” Nature, vol. 381, no. 6585, pp. 811–812, 1996. [88] L. Böhme, L. Morales-Rivas, S. Diederichs, and E. Kerscher, “Crystal c-axis mapping of hcp metals by conventional reflected polarized light microscopy: Application to untextured and textured cp-Titanium,” Materials Characterization, vol. 145, no. September, pp. 573–581, 2018. [89] L. Bartlett, Variability in coloured titanium surfaces for jewellery. PhD thesis, University of the Arts London, 2009. [90] D. Barnes, “Heat Tinting of Titanium and Titanium Alloys,” Metallography, Microstructure, and Analysis, vol. 5, no. 6, pp. 536–539, 2016. [91] M. L. Harper, Y. Kosaka, and S. P. Fox, “Titanium Metallography Using Heat Tinting,” Ti-2007 Science and Technology, pp. 785–788, 2007. [92] European Aviation Safety Agency, “Certification Specifications for Engines CS-E (2018 Amendment),” tech. rep., European Aviation Safety Agency, 2003. [93] D. Rugg, M. Dixon, and F. P. Dunne, “Effective structural unit size in titanium alloys,” Journal of Strain Analysis for Engineering Design, vol. 42, no. 4, pp. 269– 279, 2007. [94] C. Shamblen, A. Woodfield, P. Wayte, and G. Dilbert, “Titanium industry quality improvements,” in 10th World Conference on Titanium, pp. 2737–2744, 2003. [95] S. Panda, D. Banerjee, G. S. Avadhani, and S. Suwas, “A variant selection mechanism in the deformed and recrystallized � matrix of a metastable �-titanium alloy,” Philosophical Magazine Letters, vol. 98, no. 7, pp. 273–282, 2018. [96] K. Moussaoui, M. Mousseigne, J. Senatore, R. Chieragatti, and P. Lamesle, “Influence of Milling on the Fatigue Lifetime of a Ti6Al4V Titanium Alloy,” Metals, vol. 5, no. 3, pp. 1148–1162, 2015. [97] A. Jawaid, C. H. Che-Haron, and A. Abdullah, “Tool wear characteristics in turning of titanium alloy Ti-6246,” Journal of Materials Processing Technology, vol. 92-93, pp. 329–334, 1999. [98] C. J. Pretorius, S. L. Soo, D. K. Aspinwall, P. M. Harden, R. M’Saoubi, and A. L. Mantle, “Tool wear behaviour and workpiece surface integrity when turning Ti-6Al- 2Sn-4Zr-6Mo with polycrystalline diamond tooling,” CIRP Annals - Manufacturing Technology, vol. 64, no. 1, pp. 109–112, 2015. [99] C. Veiga, J. P. Davim, and A. J. R. Loureiro, “Review on machinability of titanium alloys: The process perspective,” Reviews on Advanced Materials Science, vol. 34, no. 2, pp. 148–164, 2013. [100] P. J. Arrazola, A. Garay, L. M. Iriarte, M. Armendia, S. Marya, and F. Le Maître, “Machinability of titanium alloys (Ti6Al4V and Ti555.3),” Journal of Materials Processing Technology, vol. 209, no. 5, pp. 2223–2230, 2009. [101] M. Armendia, P. Osborne, a. Garay, J. Belloso, S. Turner, and P.-J. Arrazola, “Influence of Heat Treatment on the Machinability of Titanium Alloys,” Materials and Manufacturing Processes, vol. 27, no. 4, pp. 457–461, 2012. [102] M. Thomas, S. Turner, and M. Jackson, “Microstructural damage during highspeed milling of titanium alloys,” Scripta Materialia, vol. 62, no. 5, pp. 250–253, 2010. [103] P. Crawforth, B. Wynne, S. Turner, and M. Jackson, “Subsurface deformation during precision turning of a near-alpha titanium alloy,” Scripta Materialia, vol. 67, no. 10, pp. 842–845, 2012. [104] M. Thomas, T. Lindley, D. Rugg, and M. Jackson, “The effect of shot peening on the microstructure and properties of a near-alpha titanium alloy following high temperature exposure,” Acta Materialia, vol. 60, no. 13-14, pp. 5040–5048, 2012. [105] A. Wilson, V. Venkatesh, R. Pather, J. W. Brooks, and S. Fox, “The Prediction of Microstructural Development during TIMETAL 6-4 Billet Manufacture,” in World Conference on Titanium; Ti-2003, pp. 321–328, 2003. [106] D. Suárez Fernández, B. P. Wynne, P. Crawforth, K. Fox, and M. Jackson, “A Novel Technique to Assess the Effect of Machining and Subsurface Microstructure on the Fatigue Performance of Ti-6Al-2Sn-4Zr-6Mo,” in Proceedings for the 14th World Conference on Titanium, p. (Accepted for Publication), 2019. [107] A. K. Ackerman, A. J. Knowles, H. M. Gardner, A. A. Németh, I. Bantounas, A. Radecka, M. P. Moody, P. A. Bagot, R. C. Reed, D. Rugg, and D. Dye, “The Kinetics of Primary Alpha Plate Growth in Titanium Alloys,” Metallurgical and Materials Transactions A: Physical Metallurgy and Materials Science, 2020. [108] I. Bantounas, D. Dye, and T. C. Lindley, “The effect of grain orientation on fracture morphology during high-cycle fatigue of Ti-6Al-4V,” Acta Materialia, 2009. [109] M. Hosson and A. Brebbia, “Surface Effects and Contact Mechanics IX - Computational Methods and Experiments,” 2009. [110] A. Ginting and M. Nouari, “Surface integrity of dry machined titanium alloys,” International Journal of Machine Tools and Manufacture, vol. 49, no. 3-4, pp. 325– 332, 2009. [111] B. Zou, M. Chen, C. Huang, and Q. An, “Study on surface damages caused by turning NiCr20TiAl nickel-based alloy,” Journal of Materials Processing Technology, vol. 209, no. 17, pp. 5802–5809, 2009. [112] R. S. Pawade, S. S. Joshi, P. K. Brahmankar, and M. Rahman, “An investigation of cutting forces and surface damage in high-speed turning of Inconel 718,” Journal of Materials Processing Technology, vol. 192-193, pp. 139–146, 2007. [113] A. Souto-Lebel, N. Guillemot, C. Lartigue, and R. Billardon, “Characterization and influence of defect size distribution induced by ball-end finishing milling on fatigue life,” Procedia Engineering, vol. 19, pp. 343–348, 2011. [114] M. R. Bayoumi and A. K. Abdellatif, “Effect of surface finish on fatigue strength,” Engineering Fracture Mechanics, vol. 51, no. 5, pp. 861–870, 1995. [115] D. Wilson, Z. Zheng, and F. P. Dunne, “A microstructure-sensitive driving force for crack growth,” Journal of the Mechanics and Physics of Solids, vol. 121, pp. 147– 174, 2018. [116] Z. Zheng, D. S. Balint, and F. P. Dunne, “Investigation of slip transfer across HCP grain boundaries with application to cold dwell facet fatigue,” Acta Materialia, vol. 127, pp. 43–53, 2017. [117] Z. Zheng, D. S. Balint, and F. P. Dunne, “Dwell fatigue in two Ti alloys: An integrated crystal plasticity and discrete dislocation study,” Journal of the Mechanics and Physics of Solids, vol. 96, pp. 411–427, 2016. [118] A. Stroh, “The formation of cracks as a result of plastic flow,” Proceedings of the Royal Society of London. Series A. Mathematical and Physical Sciences, pp. 404– 414, 1954. [119] F. P. Dunne and D. Rugg, “On the mechanisms of fatigue facet nucleation in titanium alloys,” Fatigue and Fracture of Engineering Materials and Structures, vol. 31, no. 11, pp. 949–958, 2008. [120] F. P. Dunne, D. Rugg, and A. Walker, “Lengthscale-dependent, elastically anisotropic, physically-based hcp crystal plasticity: Application to cold-dwell fatigue in Ti alloys,” International Journal of Plasticity, vol. 23, no. 6, pp. 1061–1083, 2007. [121] I. Bantounas, T. C. Lindley, D. Rugg, and D. Dye, “Effect of microtexture on fatigue cracking in Ti-6Al-4V,” Acta Materialia, vol. 55, no. 16, pp. 5655–5665, 2007. [122] D. Ulutan and T. Ozel, “Machining induced surface integrity in titanium and nickel alloys: A review,” International Journal of Machine Tools and Manufacture, vol. 51, no. 3, pp. 250–280, 2011. [123] A. R. Machado and J. J Wallbank, “Machining of Titanium and its Alloys—a Review,” Proceedings of the Institution of Mechanical Engineers, Part B: Journal of Engineering Manufacture, vol. 3, no. 1, pp. 107–139, 1990. [124] E. Abboud, H. Attia, B. Shi, A. Damir, V. Thomson, and Y. Mebrahtu, “Residual Stresses and Surface Integrity of Ti-alloys during Finish Turning - Guidelines for Compressive Residual Stresses,” in Procedia CIRP, 2016. [125] P. de Vos and J.-E. Stahl, Applied Metal Cutting Physics - Best Practice. Fagersta, Sweeden: SECO TOOLS, 2016. [126] E. Chiappini, S. Tirelli, P. Albertelli, M. Strano, and M. Monno, “On the mechanics of chip formation in Ti-6Al-4V turning with spindle speed variation,” International Journal of Machine Tools and Manufacture, vol. 77, pp. 16–26, 2014. [127] M. K. Dikshit, A. B. Puri, and A. Maity, “Analysis of rotational speed variations on cutting force coefficients in high-speed ball end milling,” Journal of the Brazilian Society of Mechanical Sciences and Engineering, vol. 39, no. 9, pp. 3529–3539, 2017. [128] O. Gonzalo, J. Beristain, H. Jauregi, and C. Sanz, “A method for the identification of the specific force coefficients for mechanistic milling simulation,” International Journal of Machine Tools and Manufacture, vol. 50, no. 9, pp. 765–774, 2010. [129] W. Pan, S. Ding, and J. Mo, “The prediction of cutting force in end milling titanium alloy (Ti6Al4V) with polycrystalline diamond tools,” Proceedings of the Institution of Mechanical Engineers, Part B: Journal of Engineering Manufacture, vol. 231, no. 1, pp. 3–14, 2017. [130] S. Cedergren, G. Petti, and G. Sjöberg, “On the influence of work material microstructure on chip formation, cutting forces and acoustic emission when machining Ti-6Al-4V,” Procedia CIRP, vol. 12, pp. 55–60, 2013. [131] V. Wagner, M. Baili, and G. Dessein, “The relationship between the cutting speed, tool wear, and chip formation during Ti-5553 dry cutting,” International Journal of Advanced Manufacturing Technology, vol. 76, no. 5-8, pp. 893–912, 2014. [132] S. Cedergren, C. Frangoudis, A. Archenti, R. Pederson, and G. Sjöberg, “Influence of work material microstructure on vibrations when machining cast Ti-6Al-4V,” International Journal of Advanced Manufacturing Technology, vol. 84, no. 9-12, pp. 2277–2291, 2016. [133] P. Crawforth, M. Jackson, S. Turner, and B. P. Wynne, “Linking Machining Response of Titanium Billet to Upstream Thermomechanical Processing,” Proceedings of the 13th World Conference on Titanium, pp. 1649–1654, 2016. [134] Z. J. Yuan, W. B. Lee, Y. X. Yao, and M. Zhou, “Effect of Crystallographic Orientation on Cutting Forces and Surface Quality in Diamond Cutting of Single Crystal,” CIRP Annals - Manufacturing Technology, vol. 43, no. 1, pp. 39–42, 1994. [135] W. B. Lee, S. To, and C. F. Cheung, “Effect of crystallographic orientation in diamond turning of copper single crystals,” Scripta Materialia, vol. 42, no. 10, pp. 937–945, 2000. [136] B. L. Lawson, N. Kota, and O. B. Ozdoganlar, “Effects of crystallography anistropy on orthogonal micromachining of single-crystal aluminum,” Journal of Manufacturing Science and Engineering, Transactions of the ASME, vol. 130, no. 3, 2008. [137] J. Shigley, R. Budynas, and J. K. Nisbett, Shigley’s Mechanical Engineering Design. Mc Graw Hill, ninth edit ed., 2012. [138] A. Gomez-Gallegos, P. Mandal, D. Gonzalez, N. Zuelli, and P. Blackwell, “Studies on titanium alloys for aerospace application,” Defect and Diffusion Forum, vol. 385 DDF, pp. 419–423, 2018. [139] N. Khanna, A. Garay, L. M. Iriarte, D. Soler, K. S. Sangwan, and P. J. Arrazola, “Effect of heat treatment conditions on the machinability of Ti64 and Ti54M alloys,” Procedia CIRP, vol. 1, no. 1, pp. 477–482, 2012. [140] P. Crawforth, Towards a Micromechanistic Understanding of Imparted Subsurface Deformation During Machining of Titanium Alloys. PhD thesis, The University of Sheffield, 2014. [141] Y. Mizumoto, T. Aoyama, and Y. Kakinuma, “Basic study on ultraprecision machining of single-crystal calcium fluoride,” Procedia Engineering, vol. 19, pp. 264– 269, 2011. [142] S. Abolfazl Zahedi, A. Roy, and V. V. Silberschmidt, “Variation of cutting forces in machining of f.c.c. single crystals,” Acta Mechanica, vol. 227, no. 1, pp. 3–9, 2016"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.816932"]},{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["EP/L016273"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/27926/1/CR.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Safety-critical aerospace jet engine components such as titanium alloy compressor discs are manufactured under very strict standards and regulations. It is essential that the effects of every manufacturing stage is fully understood to ensure the best performance and avoid catastrophic failures. In this study the effects of upstream forging and downstream machining were determined and correlated with the variable fatigue performance of a number of Rolls-Royce Ti-6Al-2Sn-4Zr-6Mo compressor disc forgings used in the intermediate pressure section of a gas turbine aero-engine. A four-point flexural testing approach was used to characterise the fatigue life heterogeneity at different circumferential locations in a Ti-6Al-2Sn-4Zr-6Mo compressor discs. Texture analysis using electron backscattered diffraction linked these fatigue life differences with the heterogeneous nonlinear strain pattern induced during the open die hot forging process at the primary forging stage of the VAR ingot. Moreover, this texture analysis also revealed the alignment of the HCP crystal c-axis in the radial direction parallel to the hoop stress during the close die forging secondary forging. Crack initiation analysis of fatigue test coupons of these regions were dominated with alpha phase that was orientated at an angle of 20-40o with respect to the loading direction. This demonstrated that there is no purely basal cleavage and a component of the applied stress has been transformed into deformation slip to initiate a crack. EBSD analysis was performed to understand the crack propagation mechanisms after identifying different crack path geometries during fractography analysis. Best performing circumferential regions displayed a more convoluted crack path and a lower texture index (MUD), as opposed to the straight cracks in the worst performing regions. This was directly correlated to the texture heterogeneities induced during forging. Moreover, the best performing samples showed crack diversion/arrest when the crack tip encountered regions unfavourably orientated for prismatic slip with respect to the loading direction. A small-scale machining test was developed to recreate the industrial face turning process in small samples, making it more resource efficient to test different machining parameters. This process was used to machine flat coupons, extracted from a second Ti-6Al-2Sn-4Zr-6Mo alloy forged disc, which were subsequently tested in the 4-point bend fatigue approach. This enabled the effects of machining parameters on the surface performance to be directly correlated to the fatigue life. Results showed that faster cutting speeds and metal removal rates did not have any detrimental effect on fatigue life. In fact, machined coupons presented up to three times the fatigue life compared to non-machined ones. However, circumferential variation in fatigue life was still present, suggesting that the inherent forging effects on fatigue life cannot be “erased” through the machining process. A third Ti-6Al-2Sn-4Zr-6Mo disc was machined at Rolls- Royce facilities to evaluate the capabilities of the production machines when machining at higher speeds. Vibrations in the component and mid-range speeds induced chattering which produced distinct surface markings. However, this effect was not seen at the current industry standard or fastest machining speeds. This was attributed to modal frequencies and system vibrations. Finally, force feedback analysis (FFA) has been used to characterise the microstructure of a range of titanium alloys (and heat treatment conditions) through the measured cutting forces. Heterogeneous cutting performance has been linked to the primary forging process, demonstrated in a Ti-54M forged billet, and a closer inspection of the collected signal, allowed grain size measurements and microstructural features reconstruction in ”fingerprint diagrams”. This reconstruction was validated using in a �-forged Ti-17 billet."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["An Assessment of the Effect of Machining and Forging Texture on the Fatigue Performance of Aerospace Titanium Alloys"]}]}],"canonical_facts":{"dc:contributor.advisor":["Jackson, Martin","Wynne, Bradley","Fox, Kate"],"dc:contributor.sponsor":["EPSRC"],"dc:creator":["Suárez Fernández, Daniel"],"dc:date":["2020-04"],"dc:date.issued":["2020-04"],"dc:description.abstract":["Safety-critical aerospace jet engine components such as titanium alloy compressor discs are manufactured under very strict standards and regulations. It is essential that the effects of every manufacturing stage is fully understood to ensure the best performance and avoid catastrophic failures. In this study the effects of upstream forging and downstream machining were determined and correlated with the variable fatigue performance of a number of Rolls-Royce Ti-6Al-2Sn-4Zr-6Mo compressor disc forgings used in the intermediate pressure section of a gas turbine aero-engine. A four-point flexural testing approach was used to characterise the fatigue life heterogeneity at different circumferential locations in a Ti-6Al-2Sn-4Zr-6Mo compressor discs. Texture analysis using electron backscattered diffraction linked these fatigue life differences with the heterogeneous nonlinear strain pattern induced during the open die hot forging process at the primary forging stage of the VAR ingot. Moreover, this texture analysis also revealed the alignment of the HCP crystal c-axis in the radial direction parallel to the hoop stress during the close die forging secondary forging. Crack initiation analysis of fatigue test coupons of these regions were dominated with alpha phase that was orientated at an angle of 20-40o with respect to the loading direction. This demonstrated that there is no purely basal cleavage and a component of the applied stress has been transformed into deformation slip to initiate a crack. EBSD analysis was performed to understand the crack propagation mechanisms after identifying different crack path geometries during fractography analysis. Best performing circumferential regions displayed a more convoluted crack path and a lower texture index (MUD), as opposed to the straight cracks in the worst performing regions. This was directly correlated to the texture heterogeneities induced during forging. Moreover, the best performing samples showed crack diversion/arrest when the crack tip encountered regions unfavourably orientated for prismatic slip with respect to the loading direction. A small-scale machining test was developed to recreate the industrial face turning process in small samples, making it more resource efficient to test different machining parameters. This process was used to machine flat coupons, extracted from a second Ti-6Al-2Sn-4Zr-6Mo alloy forged disc, which were subsequently tested in the 4-point bend fatigue approach. This enabled the effects of machining parameters on the surface performance to be directly correlated to the fatigue life. Results showed that faster cutting speeds and metal removal rates did not have any detrimental effect on fatigue life. In fact, machined coupons presented up to three times the fatigue life compared to non-machined ones. However, circumferential variation in fatigue life was still present, suggesting that the inherent forging effects on fatigue life cannot be “erased” through the machining process. A third Ti-6Al-2Sn-4Zr-6Mo disc was machined at Rolls- Royce facilities to evaluate the capabilities of the production machines when machining at higher speeds. Vibrations in the component and mid-range speeds induced chattering which produced distinct surface markings. However, this effect was not seen at the current industry standard or fastest machining speeds. This was attributed to modal frequencies and system vibrations. Finally, force feedback analysis (FFA) has been used to characterise the microstructure of a range of titanium alloys (and heat treatment conditions) through the measured cutting forces. Heterogeneous cutting performance has been linked to the primary forging process, demonstrated in a Ti-54M forged billet, and a closer inspection of the collected signal, allowed grain size measurements and microstructural features reconstruction in ”fingerprint diagrams”. This reconstruction was validated using in a �-forged Ti-17 billet."],"dc:format":["text"],"dc:identifier":["uk.bl.ethos.816932"],"dc:identifier.grantnumber":["EP/L016273"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/27926/1/CR.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Materials Science and Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/27926/"],"dc:relation.references":["[1] Roskill Market Reports and Consultancy, “Titanium Metal: Global Industry, Markets & Outlook,” tech. rep., Roskill, 2018. [2] N. Lecca, “Airbus commercial aircraft results 2017,” tech. rep., Airbus, 2018. [3] Airbus S.A.S. (Airbus Group), “Taking the lead: The A350XWB,” 2006. [4] J. Halford, “Driving Growth through Innovation Commercial and Military Titanium Demand Trends,” tech. rep., Arconic, Singapore, 2018. [5] E. Schulz, “Global Market Forecast: Growing Horizons 2017/2036,” Airbus Global Market Forecast, 2018. [6] N. Tian, A. Fleurant, A. Kuimova, P. Wezeman, and S. Wezeman, “Trends in World Military Expenditure, 2017,” Tech. Rep. May, Stockholm International Peace Research Institute, Stockholm, 2018. [7] S. Seong, O. Younossi, and B. W. Goldsmith, “Titanium Industrial Base, Price Trends, and Technology Initiatives,” tech. rep., RAND, 2009. [8] European Comission, “Climate Action: Reducing emissions from aviation.” [9] European Parliament, “Regulation (EU) No 598/2014 of the European Parliament and of the Council of 16 April 2014 on the establishment of rules and procedures with regard to the introduction of noise-related operating restrictions at Union airports within a Balanced Approach,” Tech. Rep. 598, European Union, 2014. [10] European Comission, “Aircraft Noise.” [11] Aviation Safety Network (Flight Safety Foundation), “Number of airliner accidents per,” 2018. [12] National Transportation Safety Board, “In Reply refer to: A-90-167 National Transportation Safety Board,” tech. rep., National Transportation Safety Board, 1990. [13] National Transportation Safety Board, “Aircraft Accident Report: United Airlines Flight 232, McDonnell Douglas DC-I0-10, Sioux Gateway Airport, Sioux City, Iowa, July 19 1989,” tech. rep., National Transportation Safety Board, 1989. [14] M. C. Blakey, “Safety Recommendation: In reply refer to: A-06-60 through -64,” tech. rep., National Transportation Safety Board, 2006. [15] National Transportation Safety Board, “Uncontained Engine Failure and Subsequent Fire, American Airlines Flight 383, Boeing 767-323, N345AN, Chicago, Illinois, October 28, 2016,” tech. rep., National Transportation Safety Board, 2016. [16] Australian Transport Safety Bureau, “In-flight uncontained engine failure A380- 842, VH-OQA,” Tech. Rep. June, Australian Transport Safety Bureau, 2013. [17] R.-R. plc, “Annual Report 2017 Rolls-Royce Holdings plc,” tech. rep., Rolls-Royce Holdings plc, 2017. [18] J. Esslinger, “Titanium in Aero Engines Demands on Titanium Alloys and Processes in Aero Engines,” Proceedings of the 10thWorld Conference on Titanium (Ti-2003), pp. 2845–2852, 2003. [19] N. S. Weston and M. Jackson, “FAST-forge − A new cost-effective hybrid processing route for consolidating titanium powder into near net shape forged components,” Journal of Materials Processing Technology, vol. 243, pp. 335–346, 2017. [20] F. Martina and S. Williams, “Wire+arc additive manufacturing vs. traditional machining from solid: a cost comparison,” tech. rep., Cranfield University, 2015. [21] B. Hurles and F. Froes, “Lowering the cost of titanium,” AMPTIAC Quarterly, vol. 6, no. 2, 2002. [22] P. Mallick, C. Horvath, J. Benedyk, B. Powell, A. Luo, P. Krajewski, G. T. Kridli, P. A. Friedman, J. M. Boileau, S. Das, and A. Deb, Materials, Design and Manufacturing for Lightweight Vehicles. CRC, 2010. [23] F. H. Froes, H. Friedrich, J. Kiese, and D. Bergoint, “Titanium in the family automobile: The cost challenge,” Cost - Affordable Titanium, Symposium, dedicated to Professor Harvey Flower, no. February 2004, pp. 159–166, 2004. [24] A. Acharya and V. A. Gokhale, “Titanium: A New Generation Material for Architectural Applications,” International Journal of Engineering Research and Applications, vol. 05, no. 02, pp. 22–29, 2015. [25] G. Lutjering and J. Williams, Engineering Materials and Processes: Titanium. Springer, 2007. [26] M. George and USGS (United States Geological Survey), “Titanium and Titanium Dioxide (USGS),” tech. rep., United States Geological Survey, 2020. [27] A. Zarkades and F. Larson, “Elasticity of Titanium Sheet Alloys,” in The Science, Technology and Application of Titanium, pp. 933–941, Pergamon Press Ltd, 1970. [28] G. Lütjering and J. C. Williams, Titanium Book. Springer, 2007. [29] M. J. Donachie, Titanium - A Technical Guide. ASM International, 2000. [30] R. R. Boyer, “Aerospace applications of beta titanium alloys,” Jom, vol. 46, no. 7, pp. 20–23, 1994. [31] TIMET Ltd., “Timetal 6-2-4-6 Mechanical Properties,” 2019. [32] T. Krull, J. Albrecht, and G. Lüetjering, “The Effect of Yield Stress Level on the Mechanical Properties of Ti-6246,” Science and Technology, The Japan Institute of Metals, pp. 519–522, 2007. [33] S. Kathleen, S. Dragolich, N. D. DiMatteo, and S. D. Henry, Fatigue Data Book: Light Structural Alloys. ASM (American Society of Metals), 1994. [34] C. E. W. Boyer R., Welsch G., Materials Properties Handbook: Titanium Alloys. ASM International, 1994. [35] SAE Aerospace, “Aerospace Material Specification SAE AMS 4981E, Titanium Alloy Bars, Wire, and Forgings 6.0Al - 2.0Sn - 4.0Zr - 6.0Mo Solution and Precipitation Heat Treated,” 2006. [36] D. R. N. Correa, F. B. Vicente, R. O. Araújo, M. L. Lourenço, P. A. B. Kuroda, M. A. R. Buzalaf, and C. R. Grandini, “Effect of the substitutional elements on the microstructure of the Ti-15Mo-Zr and Ti-15Zr-Mo systems alloys,” Journal of Materials Research and Technology, vol. 4, no. 2, pp. 180–185, 2015. [37] A. Banerjee, S. Balachandran, S. Suwas, and D. Banerjee, “Deformation Behaviour of Titanium Alloys Ti-6242 and Ti-6246,” Proceedings of the 13th World Conference on Titanium, no. Table I, pp. 1095–1101, 2016. [38] R. Wanhill and S. Barter, Fatigue of Beta Processed and Beta Heat-treated Titanium Alloys. Springer Science and Business Media, 2011. [39] S. Hémery and P. Villechaise, “Comparison of slip system activation in Ti-6Al-2Sn- 4Zr-2Mo and Ti-6Al-2Sn-4Zr-6Mo under tensile, fatigue and dwell-fatigue loadings,” Materials Science and Engineering A, vol. 697, no. March, pp. 177–183, 2017. [40] I. Inagaki, T. Takechi, S. Yoshihisa, and A. Nozomu, “Application and Features of Titanium for the Aerospace Industry,” Nippon Steel & Sumitomo Metal Technical Report, no. 106, pp. 22–27, 2014. [41] D. Eylon, S. Fujishiro, and F. H. Froes, “Titanium Alloys for High Temperature Applications — a Review,” High Temperature Materials and Processes, vol. 6, no. 1- 2, pp. 81–92, 1984. [42] M. Evans and A. R. Ward, “Corrosion resistance of Ti-6246 for high power aeroengine compressor discs and blades,” Materials Science and Technology, vol. 17, no. 8, pp. 945–953, 2001. [43] S. Joseph, T. C. Lindley, D. Dye, and E. A. Saunders, “The mechanisms of hot salt stress corrosion cracking in titanium alloy Ti-6Al-2Sn-4Zr-6Mo,” Corrosion Science, vol. 134, pp. 169–178, 2018. [44] D. Banerjee and J. C. Williams, “Perspectives on titanium science and technology,” Acta Materialia, vol. 61, no. 3, pp. 844–879, 2013. [45] Z. Zheng, D. S. Balint, and F. P. E. Dunne, “Dwell fatigue in two Ti alloys: An integrated crystal plasticity and discrete dislocation study,” Journal of the Mechanics and Physics of Solids, vol. 96, pp. 411–427, 2016. [46] M. R. Bache, M. Cope, H. M. Davies, W. J. Evans, and G. Harrison, “Dwell sensitive fatigue in a near alpha titanium alloy at ambient temperature,” International Journal of Fatigue, vol. 19, no. SUPPL.1, pp. 83–88, 1997. [47] J. Qiu, Y. Ma, J. Lei, Y. Liu, A. Huang, D. Rugg, and R. Yang, “A Comparative Study on Dwell Fatigue of Ti-6Al-2Sn-4Zr-xMo (x = 2 to 6) Alloys on a Microstructure-Normalized Basis,” Metallurgical and Materials Transactions A: Physical Metallurgy and Materials Science, vol. 45, no. 13, pp. 6075–6087, 2014. [48] R. B. Osman and M. V. Swain, “A critical review of dental implant materials with an emphasis on titanium versus zirconia,” Materials, vol. 8, no. 3, pp. 932–958, 2015. [49] C. Leyens and M. Peters, Titanium and Titanium Alloys. Wiley-VCH, 2003. [50] D. Williams, “The effects of zirconium in titanium-base alloys,” Journal of less common metals, vol. 6, pp. 219–225, 1964. [51] D. R. N. Correa, F. B. Vicente, T. A. G. Donato, V. E. Arana-Chavez, M. A. R. Buzalaf, and C. R. Grandini, “The effect of the solute on the structure, selected mechanical properties, and biocompatibility of Ti-Zr system alloys for dental applications,” Materials Science and Engineering C, vol. 34, no. 1, pp. 354–359, 2014. [52] W. G. Burgers, “W.G. Burgers Physica 1934.pdf,” Physica, vol. 1, no. 7-12, pp. 549– 560, 1933. [53] V. Tong, S. Joseph, A. K. Ackerman, D. Dye, and T. B. Britton, “Using transmission Kikuchi diffraction to characterise alpha variants in an alpha + beta titanium alloy,” Journal of Microscopy, vol. 267, no. 3, pp. 318–329, 2016. [54] T. B. Britton, J. Jiang, Y. Guo, A. Vilalta-Clemente, D. Wallis, L. N. Hansen, A. Winkelmann, and A. J. Wilkinson, “Tutorial: Crystal orientations and EBSD - Or which way is up?,” Materials Characterization, vol. 117, pp. 113–126, 2016. [55] M. G. Glavicic, B. B. Bartha, S. K. Jha, and C. J. Szczepanski, “The origins of microtexture in duplex Ti alloys,” Materials Science and Engineering A, vol. 513- 514, no. C, pp. 325–328, 2009. [56] E. Lee, R. Banerjee, S. Kar, D. Bhattacharyya, and H. L. Fraser, “Selection of � variants during microstructural evolution in �/� titanium alloys,” Philosophical Magazine, vol. 87, no. 24, pp. 3615–3627, 2007. [57] J. Walter, M. Jackson, and C. Sims, Titanium and its alloys: Principles of Alloying Titanium. ASM International, 1988. [58] G. Lütjering, “Influence of processing on microstructure and mechanical properties of (� + �) titanium alloys,” Materials Science and Engineering A, vol. 243, no. 1-2, pp. 32–45, 1998. [59] J. B. Borradaile and R. H. Heal, “Critical Review Mechanical Properties of Titanium Alloys,” Proc. Titanium, vol. 1, pp. 141–152, 1980. [60] T. Choda, H. Oyama, and S. Murakami, “Technology for process design of titanium alloy forging,” Journal of Japan Institute of Light Metals, vol. 65, no. 9, pp. 460–465, 2015. [61] Z. Z. Fang, J. D. Paramore, P. Sun, K. S. Chandran, Y. Zhang, Y. Xia, F. Cao, M. Koopman, and M. Free, “Powder metallurgy of titanium–past, present, and future,” International Materials Reviews, vol. 63, no. 7, pp. 407–459, 2018. [62] C. Brooks, Heat treatment, structure and properties of nonferrous alloys. ASM (American Society of Metals), 1982. [63] J. Xu, Z. Zhang, P. Fang, and W. Hu, “Summary Abstract: Comparison of ingot structure of vacuum arc remelting–vacuum arc double‐electrode remelting processes: Study of the possibility of using cast titanium directly as an isothermo‐forging billet,” Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films, vol. 5, no. 4, pp. 2682–2683, 1987. [64] R. C. Atwood, P. D. Lee, R. S. Minisandram, and R. M. Jones, “Multiscale modelling of microstructure formation during vacuum arc remelting of titanium 6-4,” Journal of Materials Science, vol. 39, no. 24, pp. 7193–7197, 2004. [65] I. Weiss and S. L. Semiatin, “Thermomechanical processing of alpha titanium alloys - An overview,” Materials Science and Engineering A, vol. 263, no. 2, pp. 243–256, 1999. [66] J. D. Cotton, R. D. Briggs, R. R. Boyer, S. Tamirisakandala, P. Russo, N. Shchetnikov, and J. C. Fanning, “State of the Art in Beta Titanium Alloys for Airframe Applications,” Jom, vol. 67, no. 6, pp. 1281–1303, 2015. [67] Z. Guo and T. Baker, “On the microstructure and thermomechanical processing of titanium alloy IMI685,” Materials Science and Engineering A, vol. 1, no. 1, pp. 63–76, 1992. [68] P. Davies, An Investigation of Microstructure and Texture Evolution in the Near-� Titanium Alloy Timetal 834. PhD thesis, The University of Sheffield, 2009. [69] P. Partridge, “The crystallography and deformation modes of hexagonal closepacked metals,” Metallurgical Reviews, vol. 6690, pp. 169–194, 1967. [70] M. H. Yoo, “Slip, twinning, and fracture in hexagonal close-packed metals,” Metallurgical Transactions A, vol. 12, no. 3, pp. 409–418, 1981. [71] D. G. R. William D. Callister, Jr., Materials Science and Engineering An introduction, vol. 1. John Wiley & Sons, 8th ed., 2010. [72] S. L. Semiatin, T. R. Bieler, and I. Introduction, “Effect of Texture and Slip Mode on the Anisotropy of Plastic Flow and Flow Softening during Hot Working of Ti- 6Al-4V,” Metallurgical and Materials Transactions A: Physical Metallurgy and Materials Science, vol. 32, no. July, 2001. [73] Y. C. Lin, B. H. Yan, and Y. S. Chang, “Machining characteristics of titanium alloy (Ti-6Al-4V) using a combination process of EDM with USM,” Journal of Materials Processing Technology, vol. 104, no. 3, pp. 171–177, 2000. [74] S. Kuriakose and M. S. Shunmugam, “Characteristics of wire-electro discharge machined Ti6Al4V surface,” Materials Letters, vol. 58, no. 17-18, pp. 2231–2237, 2004. [75] T. Ahmed and H. J. Rack, “Phase transformations during cooling in alpha + beta titanium alloys,” 1998. [76] A. Hasçalik and U. Çaydaş, “Electrical discharge machining of titanium alloy (Ti- 6Al-4V),” Applied Surface Science, vol. 253, no. 22, pp. 9007–9016, 2007. [77] F. Klocke, D. Welling, and J. Dieckmann, “Comparison of grinding and Wire EDM concerning fatigue strength and surface integrity of machined Ti6Al4V components,” Procedia Engineering, vol. 19, no. December 2011, pp. 184–189, 2011. [78] M. Manjaiah, S. Narendranath, and S. Basavarajappa, “A Reviwe on Machining of Titanium Based Alloys Using EDM and WEDM,” Reviews on advanced materials science, vol. 36, pp. 89–111, 2014. [79] ASTM, “Standard Test Method for Strain-Controlled Fatigue Testing,” Tech. Rep. 2004, ASTM, 2004. [80] ASTM, “Astm E399,” tech. rep., ASTM, 2016. [81] ASTM, “ASTM D790-03.Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials.American Society for Testing and Materials. United States of America,” tech. rep., ASTM, 2017. [82] A. Cox, Understanding the effect of surface generation rates for finish milling of aero-structural components. PhD thesis, The University of Sheffield, 2017. [83] A. Cox, S. Herbert, J. P. Villain-Chastre, S. Turner, and M. Jackson, “The effect of machining and induced surface deformation on the fatigue performance of a high strength metastable � titanium alloy,” International Journal of Fatigue, vol. 124, no. February, pp. 26–33, 2019. [84] M. Whittaker, Titanium in the Gas Turbine Engine. INTECH, 2011. [85] D. Tromans, “Elastic Anisotropy of HCP Metal Crystals and Polycrystals,” Ijrras, vol. 6, no. March, pp. 462–483, 2011. [86] R. Weaver, “Rediscovering Polarized Light Microscopy,” Tech. Rep. October, AMERICAN LABORATORY, 2003. [87] R. Oldenbourg, “A new view on polarization microscopy.,” Nature, vol. 381, no. 6585, pp. 811–812, 1996. [88] L. Böhme, L. Morales-Rivas, S. Diederichs, and E. Kerscher, “Crystal c-axis mapping of hcp metals by conventional reflected polarized light microscopy: Application to untextured and textured cp-Titanium,” Materials Characterization, vol. 145, no. September, pp. 573–581, 2018. [89] L. Bartlett, Variability in coloured titanium surfaces for jewellery. PhD thesis, University of the Arts London, 2009. [90] D. Barnes, “Heat Tinting of Titanium and Titanium Alloys,” Metallography, Microstructure, and Analysis, vol. 5, no. 6, pp. 536–539, 2016. [91] M. L. Harper, Y. Kosaka, and S. P. Fox, “Titanium Metallography Using Heat Tinting,” Ti-2007 Science and Technology, pp. 785–788, 2007. [92] European Aviation Safety Agency, “Certification Specifications for Engines CS-E (2018 Amendment),” tech. rep., European Aviation Safety Agency, 2003. [93] D. Rugg, M. Dixon, and F. P. Dunne, “Effective structural unit size in titanium alloys,” Journal of Strain Analysis for Engineering Design, vol. 42, no. 4, pp. 269– 279, 2007. [94] C. Shamblen, A. Woodfield, P. Wayte, and G. Dilbert, “Titanium industry quality improvements,” in 10th World Conference on Titanium, pp. 2737–2744, 2003. [95] S. Panda, D. Banerjee, G. S. Avadhani, and S. Suwas, “A variant selection mechanism in the deformed and recrystallized � matrix of a metastable �-titanium alloy,” Philosophical Magazine Letters, vol. 98, no. 7, pp. 273–282, 2018. [96] K. Moussaoui, M. Mousseigne, J. Senatore, R. Chieragatti, and P. Lamesle, “Influence of Milling on the Fatigue Lifetime of a Ti6Al4V Titanium Alloy,” Metals, vol. 5, no. 3, pp. 1148–1162, 2015. [97] A. Jawaid, C. H. Che-Haron, and A. Abdullah, “Tool wear characteristics in turning of titanium alloy Ti-6246,” Journal of Materials Processing Technology, vol. 92-93, pp. 329–334, 1999. [98] C. J. Pretorius, S. L. Soo, D. K. Aspinwall, P. M. Harden, R. M’Saoubi, and A. L. Mantle, “Tool wear behaviour and workpiece surface integrity when turning Ti-6Al- 2Sn-4Zr-6Mo with polycrystalline diamond tooling,” CIRP Annals - Manufacturing Technology, vol. 64, no. 1, pp. 109–112, 2015. [99] C. Veiga, J. P. Davim, and A. J. R. Loureiro, “Review on machinability of titanium alloys: The process perspective,” Reviews on Advanced Materials Science, vol. 34, no. 2, pp. 148–164, 2013. [100] P. J. Arrazola, A. Garay, L. M. Iriarte, M. Armendia, S. Marya, and F. Le Maître, “Machinability of titanium alloys (Ti6Al4V and Ti555.3),” Journal of Materials Processing Technology, vol. 209, no. 5, pp. 2223–2230, 2009. [101] M. Armendia, P. Osborne, a. Garay, J. Belloso, S. Turner, and P.-J. Arrazola, “Influence of Heat Treatment on the Machinability of Titanium Alloys,” Materials and Manufacturing Processes, vol. 27, no. 4, pp. 457–461, 2012. [102] M. Thomas, S. Turner, and M. Jackson, “Microstructural damage during highspeed milling of titanium alloys,” Scripta Materialia, vol. 62, no. 5, pp. 250–253, 2010. [103] P. Crawforth, B. Wynne, S. Turner, and M. Jackson, “Subsurface deformation during precision turning of a near-alpha titanium alloy,” Scripta Materialia, vol. 67, no. 10, pp. 842–845, 2012. [104] M. Thomas, T. Lindley, D. Rugg, and M. Jackson, “The effect of shot peening on the microstructure and properties of a near-alpha titanium alloy following high temperature exposure,” Acta Materialia, vol. 60, no. 13-14, pp. 5040–5048, 2012. [105] A. Wilson, V. Venkatesh, R. Pather, J. W. Brooks, and S. Fox, “The Prediction of Microstructural Development during TIMETAL 6-4 Billet Manufacture,” in World Conference on Titanium; Ti-2003, pp. 321–328, 2003. [106] D. Suárez Fernández, B. P. Wynne, P. Crawforth, K. Fox, and M. Jackson, “A Novel Technique to Assess the Effect of Machining and Subsurface Microstructure on the Fatigue Performance of Ti-6Al-2Sn-4Zr-6Mo,” in Proceedings for the 14th World Conference on Titanium, p. (Accepted for Publication), 2019. [107] A. K. Ackerman, A. J. Knowles, H. M. Gardner, A. A. Németh, I. Bantounas, A. Radecka, M. P. Moody, P. A. Bagot, R. C. Reed, D. Rugg, and D. Dye, “The Kinetics of Primary Alpha Plate Growth in Titanium Alloys,” Metallurgical and Materials Transactions A: Physical Metallurgy and Materials Science, 2020. [108] I. Bantounas, D. Dye, and T. C. Lindley, “The effect of grain orientation on fracture morphology during high-cycle fatigue of Ti-6Al-4V,” Acta Materialia, 2009. [109] M. Hosson and A. Brebbia, “Surface Effects and Contact Mechanics IX - Computational Methods and Experiments,” 2009. [110] A. Ginting and M. Nouari, “Surface integrity of dry machined titanium alloys,” International Journal of Machine Tools and Manufacture, vol. 49, no. 3-4, pp. 325– 332, 2009. [111] B. Zou, M. Chen, C. Huang, and Q. An, “Study on surface damages caused by turning NiCr20TiAl nickel-based alloy,” Journal of Materials Processing Technology, vol. 209, no. 17, pp. 5802–5809, 2009. [112] R. S. Pawade, S. S. Joshi, P. K. Brahmankar, and M. Rahman, “An investigation of cutting forces and surface damage in high-speed turning of Inconel 718,” Journal of Materials Processing Technology, vol. 192-193, pp. 139–146, 2007. [113] A. Souto-Lebel, N. Guillemot, C. Lartigue, and R. Billardon, “Characterization and influence of defect size distribution induced by ball-end finishing milling on fatigue life,” Procedia Engineering, vol. 19, pp. 343–348, 2011. [114] M. R. Bayoumi and A. K. Abdellatif, “Effect of surface finish on fatigue strength,” Engineering Fracture Mechanics, vol. 51, no. 5, pp. 861–870, 1995. [115] D. Wilson, Z. Zheng, and F. P. Dunne, “A microstructure-sensitive driving force for crack growth,” Journal of the Mechanics and Physics of Solids, vol. 121, pp. 147– 174, 2018. [116] Z. Zheng, D. S. Balint, and F. P. Dunne, “Investigation of slip transfer across HCP grain boundaries with application to cold dwell facet fatigue,” Acta Materialia, vol. 127, pp. 43–53, 2017. [117] Z. Zheng, D. S. Balint, and F. P. Dunne, “Dwell fatigue in two Ti alloys: An integrated crystal plasticity and discrete dislocation study,” Journal of the Mechanics and Physics of Solids, vol. 96, pp. 411–427, 2016. [118] A. Stroh, “The formation of cracks as a result of plastic flow,” Proceedings of the Royal Society of London. Series A. Mathematical and Physical Sciences, pp. 404– 414, 1954. [119] F. P. Dunne and D. Rugg, “On the mechanisms of fatigue facet nucleation in titanium alloys,” Fatigue and Fracture of Engineering Materials and Structures, vol. 31, no. 11, pp. 949–958, 2008. [120] F. P. Dunne, D. Rugg, and A. Walker, “Lengthscale-dependent, elastically anisotropic, physically-based hcp crystal plasticity: Application to cold-dwell fatigue in Ti alloys,” International Journal of Plasticity, vol. 23, no. 6, pp. 1061–1083, 2007. [121] I. Bantounas, T. C. Lindley, D. Rugg, and D. Dye, “Effect of microtexture on fatigue cracking in Ti-6Al-4V,” Acta Materialia, vol. 55, no. 16, pp. 5655–5665, 2007. [122] D. Ulutan and T. Ozel, “Machining induced surface integrity in titanium and nickel alloys: A review,” International Journal of Machine Tools and Manufacture, vol. 51, no. 3, pp. 250–280, 2011. [123] A. R. Machado and J. J Wallbank, “Machining of Titanium and its Alloys—a Review,” Proceedings of the Institution of Mechanical Engineers, Part B: Journal of Engineering Manufacture, vol. 3, no. 1, pp. 107–139, 1990. [124] E. Abboud, H. Attia, B. Shi, A. Damir, V. Thomson, and Y. Mebrahtu, “Residual Stresses and Surface Integrity of Ti-alloys during Finish Turning - Guidelines for Compressive Residual Stresses,” in Procedia CIRP, 2016. [125] P. de Vos and J.-E. Stahl, Applied Metal Cutting Physics - Best Practice. Fagersta, Sweeden: SECO TOOLS, 2016. [126] E. Chiappini, S. Tirelli, P. Albertelli, M. Strano, and M. Monno, “On the mechanics of chip formation in Ti-6Al-4V turning with spindle speed variation,” International Journal of Machine Tools and Manufacture, vol. 77, pp. 16–26, 2014. [127] M. K. Dikshit, A. B. Puri, and A. Maity, “Analysis of rotational speed variations on cutting force coefficients in high-speed ball end milling,” Journal of the Brazilian Society of Mechanical Sciences and Engineering, vol. 39, no. 9, pp. 3529–3539, 2017. [128] O. Gonzalo, J. Beristain, H. Jauregi, and C. Sanz, “A method for the identification of the specific force coefficients for mechanistic milling simulation,” International Journal of Machine Tools and Manufacture, vol. 50, no. 9, pp. 765–774, 2010. [129] W. Pan, S. Ding, and J. Mo, “The prediction of cutting force in end milling titanium alloy (Ti6Al4V) with polycrystalline diamond tools,” Proceedings of the Institution of Mechanical Engineers, Part B: Journal of Engineering Manufacture, vol. 231, no. 1, pp. 3–14, 2017. [130] S. Cedergren, G. Petti, and G. Sjöberg, “On the influence of work material microstructure on chip formation, cutting forces and acoustic emission when machining Ti-6Al-4V,” Procedia CIRP, vol. 12, pp. 55–60, 2013. [131] V. Wagner, M. Baili, and G. Dessein, “The relationship between the cutting speed, tool wear, and chip formation during Ti-5553 dry cutting,” International Journal of Advanced Manufacturing Technology, vol. 76, no. 5-8, pp. 893–912, 2014. [132] S. Cedergren, C. Frangoudis, A. Archenti, R. Pederson, and G. Sjöberg, “Influence of work material microstructure on vibrations when machining cast Ti-6Al-4V,” International Journal of Advanced Manufacturing Technology, vol. 84, no. 9-12, pp. 2277–2291, 2016. [133] P. Crawforth, M. Jackson, S. Turner, and B. P. Wynne, “Linking Machining Response of Titanium Billet to Upstream Thermomechanical Processing,” Proceedings of the 13th World Conference on Titanium, pp. 1649–1654, 2016. [134] Z. J. Yuan, W. B. Lee, Y. X. Yao, and M. Zhou, “Effect of Crystallographic Orientation on Cutting Forces and Surface Quality in Diamond Cutting of Single Crystal,” CIRP Annals - Manufacturing Technology, vol. 43, no. 1, pp. 39–42, 1994. [135] W. B. Lee, S. To, and C. F. Cheung, “Effect of crystallographic orientation in diamond turning of copper single crystals,” Scripta Materialia, vol. 42, no. 10, pp. 937–945, 2000. [136] B. L. Lawson, N. Kota, and O. B. Ozdoganlar, “Effects of crystallography anistropy on orthogonal micromachining of single-crystal aluminum,” Journal of Manufacturing Science and Engineering, Transactions of the ASME, vol. 130, no. 3, 2008. [137] J. Shigley, R. Budynas, and J. K. Nisbett, Shigley’s Mechanical Engineering Design. Mc Graw Hill, ninth edit ed., 2012. [138] A. Gomez-Gallegos, P. Mandal, D. Gonzalez, N. Zuelli, and P. Blackwell, “Studies on titanium alloys for aerospace application,” Defect and Diffusion Forum, vol. 385 DDF, pp. 419–423, 2018. [139] N. Khanna, A. Garay, L. M. Iriarte, D. Soler, K. S. Sangwan, and P. J. Arrazola, “Effect of heat treatment conditions on the machinability of Ti64 and Ti54M alloys,” Procedia CIRP, vol. 1, no. 1, pp. 477–482, 2012. [140] P. Crawforth, Towards a Micromechanistic Understanding of Imparted Subsurface Deformation During Machining of Titanium Alloys. PhD thesis, The University of Sheffield, 2014. [141] Y. Mizumoto, T. Aoyama, and Y. Kakinuma, “Basic study on ultraprecision machining of single-crystal calcium fluoride,” Procedia Engineering, vol. 19, pp. 264– 269, 2011. [142] S. Abolfazl Zahedi, A. Roy, and V. V. Silberschmidt, “Variation of cutting forces in machining of f.c.c. single crystals,” Acta Mechanica, vol. 227, no. 1, pp. 3–9, 2016"],"dcterms:accessrights":["public"],"dc:title":["An Assessment of the Effect of Machining and Forging Texture on the Fatigue Performance of Aerospace Titanium Alloys"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"],"person:identifier.orcid":["0000000151998761"]},"updated_at":"2026-11-18T22:40:18Z"}