{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:28596"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:28596","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Welding of carbide-free bainitic steels for railway applications","abstract":"Carbide Free Bainitic (CFB) steels B360 and B320 show an outstanding behaviour in terms of fatigue deformation mechanisms, mainly when analysing its resistance to head checks. This, results in a lower necessity for maintenance and therefore, in a reduction of costs. However, problems have been encountered when welding CFB rails, showing cracks when in track, in both the entry and the exit site of the weld. The mechanisms of failure of these rails is not entirely clear. Nowadays, with the rise in use of high-speed trains and high loads, Continuously Welded Rails (CWR) are gaining importance; as other joining mechanisms such as fish-plates are becoming obsolete. Almost 90% of the CWR are welded by Flash Butt Welding (FBW); which is known as one of the most reliable welding processes; nevertheless, the welds are a weak link between rails due to mechanical and microstructural variations with the parent rail. Welding of conventional pearlitic rail steels, has been under investigation on numerous occasions; however, the same has not been made as extensively on CFB rail steels. On this thesis, an extensive examination of the Heat Affected Zone (HAZ) of three FBW rails (B360, B320 and R260) is discussed. CFB FBWs showed much wider HAZ extension than conventional pearlitic steels, of importance will be the extension of the tempered or Subcritical HAZ (SCHAZ), as CFBs, mainly B360 has shown low resistance to tempering; which could result on preferential wear and plastic deformation in track applications. With the purpose of reducing the extension of the tempered SCHAZ, weld trials were carried out on B360 rails using a stationary FBW GAAS 80 / 580 Schlatter welding machine in Scunthorpe, UK. Those, were produced by variations on the number of Pre-Heat (PH) cycles, on the preheating time (s) (ON) and delay period (s) (OFF) and additions of Post Weld Heat Pulses (PWHP) at the end of the welds. Finally, an analysis of the welded rails mechanical properties was made.","abstract_html":"Carbide Free Bainitic (CFB) steels B360 and B320 show an outstanding behaviour in terms of fatigue deformation mechanisms, mainly when analysing its resistance to head checks. This, results in a lower necessity for maintenance and therefore, in a reduction of costs. However, problems have been encountered when welding CFB rails, showing cracks when in track, in both the entry and the exit site of the weld. The mechanisms of failure of these rails is not entirely clear. Nowadays, with the rise in use of high-speed trains and high loads, Continuously Welded Rails (CWR) are gaining importance; as other joining mechanisms such as fish-plates are becoming obsolete. Almost 90% of the CWR are welded by Flash Butt Welding (FBW); which is known as one of the most reliable welding processes; nevertheless, the welds are a weak link between rails due to mechanical and microstructural variations with the parent rail. Welding of conventional pearlitic rail steels, has been under investigation on numerous occasions; however, the same has not been made as extensively on CFB rail steels. On this thesis, an extensive examination of the Heat Affected Zone (HAZ) of three FBW rails (B360, B320 and R260) is discussed. CFB FBWs showed much wider HAZ extension than conventional pearlitic steels, of importance will be the extension of the tempered or Subcritical HAZ (SCHAZ), as CFBs, mainly B360 has shown low resistance to tempering; which could result on preferential wear and plastic deformation in track applications. With the purpose of reducing the extension of the tempered SCHAZ, weld trials were carried out on B360 rails using a stationary FBW GAAS 80 / 580 Schlatter welding machine in Scunthorpe, UK. Those, were produced by variations on the number of Pre-Heat (PH) cycles, on the preheating time (s) (ON) and delay period (s) (OFF) and additions of Post Weld Heat Pulses (PWHP) at the end of the welds. Finally, an analysis of the welded rails mechanical properties was made.","abstract_has_math":false,"creators":["Muniz-Mangas, Marta"],"institution":"University of Sheffield","degree_name":"Eng.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Palmiere, Eric J","Smith, Lindsey"],"committee_chairs":[],"committee_members":[],"year":2021,"date_issued":"2021-03","date_published":"2021-03","updated_at":"2026-11-18T22:41:49Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/28596/1/Welding%20of%20carbide%20free%20bainitic%20steels%20for%20railway%20applications_%20final%20submission_MMM.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A28596","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Palmiere, Eric J","Smith, Lindsey"]},{"key":"dc:creator","label":"Author","values":["Muniz-Mangas, Marta"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2021-03"]},{"key":"dc:date.issued","label":"Date","values":["2021-03"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Faculty of Engineering (Sheffield)","Materials Science and Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/28596/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["[1] R. A. Smith, “Rolling Contact Fatigue of Rails: What Remains to be Done?,” China Railw. Serv., vol. 3, p. 001, 2002. [2] U. Zerbst, R. Lundén, K.-O. Edel, and R. A. Smith, “Introduction to the damage tolerance behaviour of railway rails – a review,” Eng. Fract. Mech., vol. 76, no. 17, pp. 2563–2601, Nov. 2009 [3] R. Sawley, K. & REIFF, “Rail failure assessment for the office of the rail regulator. An assessment of rail track’s methods for managing broken and defective rails. Report of the transportation Technology centre, Colorado, USA,” 2020. [4] H. Smith, “Bainitic rail steels- By private comunication- British Steel,” 2008. [5] V. A. Profidillis, Railway engineering. Brookfield, USA: Avebury Technical, 1995. [6] C. E. Volos, “Interaction between superstructure and substructure in railways,” Concrete, no. 5, pp. 2–9, 2010. [7] Chandra Satish and Agarwal M.M., “Railway Engineering (2nd Edition),” Oxford Univ. Press, vol. 20, pp. 1–2, 2015 [8] T. C. Abadi, “Effect of sleeper and ballast interventions on rail track performance,” University of Southampton, 2015. [9] S. Iwnicki, “Future trends in railway engineering,” Proc. Inst. Mech. Eng. Part C J. Mech. Eng. Sci., vol. 223, pp. 2743–2750, 2009 [10] D. Bilow and G. Randich, “Slab track for the next 100 years,” Am. Railw. Eng. Maintenance-of-w. Assoc. - Proc. 2000 Annu. Conf., no. 1, pp. 1–20, 2000. [11] Y. Bezin, D. Farrington, C. Penny, B. Temple, and S. Iwnicki, “The dynamic response of slab track constructions and their benefit with respect to conventional ballasted track,” Veh. Syst. Dyn., vol. 48, no. SUPPL. 1, pp. 175–193, 2010 [12] D. Campbell, J. Brougham, and R. Caldwell, “Uncovering and Understanding Australia’s First Railway,” Aust. J. Multi-Disciplinary Eng., vol. 7, no. 2, pp. 147–156, 2017 [13] J. Fernández, L. Museo, and D. Ferrocarril De Asturias, “Del Hierro Al Acero: La Producción De Duro Para La Compañía Del Noroeste Los Primeros Carriles Fabricados En España,” pp. 1–12, [14] R. I. Carroll, “Surface Metallurgy and Rolling Contact Fatigue of Rail,” University of Sheffield, 2005. [15] J. Locke, “The advent of the steel rail 1857-1914,” J. Transp. Hist., pp. 18–31, 1914. [16] A. S. J. A. Z. Jilabi, “Welding of Rail Steels,” University of Manchester, 2015. [17] P. Connor, “Track basics,” Railway Technical Website, no. 2, pp. 1–13. [18] EN13674-1 European standard UIC60/60E1 900A railway steel rail. . [19] U. Olofsson and T. Telliskivi, “Wear, plastic deformation and friction of two rail steels - A full-scale test and a laboratory study,” Wear, vol. 254, no. 1–2, pp. 80–93, 2003 [20] E. Sheinman, “Wear of rails. A review of the American press,” J. Frict. Wear, vol. 33, no. 4, pp. 308–314, 2012 [21] K. M. Lee and A. A. Polycarpou, “Wear of conventional pearlitic and improved bainitic rail steels,” Wear, vol. 259, no. 1–6, pp. 391–399, Jul. 2005 [22] S. Fretwell-smith, R. Steel, and D. Driver, “Rail Degradation Mechanisms - British Steel- By private communication,” 2012. [23] E. Magel, P. Sroba, K. Sawley, and J. Kalousek, “Control of rolling contact fatigue of rails,” Cent. Surf. Transp. Technol., pp. 1–29, 2005 [24] J. E. Garnham, D. I. Fletcher, C. L. Davis, and F. J. Franklin, “Visualization and modelling to understand rail rolling contact fatigue cracks in three dimensions,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 225, no. 2, pp. 165–178, 2011 [25] H. M. Smith, “Bainitic presentation February 2011- British Steel- By private communication.” 2011 . [26] T. Mount and H. Street, “Squats and squat-type defects in rails : the understanding to date,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, pp. 235–242, 2011 [27] L. J. Drewett, “The Measurement of Residual Stresses - British Steel- By private communication,” 2001. [28] H. Xiao, Q. Chen, E. Shao, D. Wu, Z. Chen, and Z. Wang, “The effect of shot peening on rolling contact fatigue behaviour and its crack initiation and propagation in carburized steel,” Wear, vol. 151, no. 1, pp. 77–86, 1991 [29] H. M. Smith, “The bainitic rail steel - Key property requirements - British Steel- By private communication,” 1998. [30] J. Jaiswal and C. Rail, “CORUS PREMIUM GRADES TO ADRESS WEAR - British Steel - By private communication.” [31] A. C. Athukorala, D. V. De Pellegrin, and K. I. Kourousis, “Characterisation of head-hardened rail steel in terms of cyclic plasticity response and microstructure for improved material modelling,” Wear, vol. 366–367, pp. 416–424, 2016 [32] H. K. D. H. Bhadeshia, “Bainite in Steels,” 2001. [33] J. Kalousek, D. M. Fegredo, and E. E. Laufer, “The wear resistance and worn metallography of pearlite, bainite and tempered martensite rail steel microstructures of high hardness,” Wear, vol. 105, pp. 199–222, 1985. [34] P. Clayton and N. Jin, “Unlubricated sliding and rolling/sliding wear behavior of continuously cooled, low/medium carbon bainitic steels,” Wear, vol. 200, no. 1–2, pp. 74–82, Dec. 1996 [35] H. K. D. H. Bhadeshia and D. V. Edmonds, “Bainite in silicon steels: new composition–property approach Part 1,” Met. Sci., vol. 17, no. September, pp. 420–425, 1983, doi: 10.1179/030634583790420646. [36] H. K. D. H. Bhadeshia, “Some phase transformations in steels,” Mater. Sci. Technol., vol. 0836, no. 1999, 2013 [37] Y. T. Chi, Y. T. Tsai, B. M. Huang, and J. R. Yang, “Investigation of idiomorphic ferrite and allotriomorphic ferrite using electron backscatter diffraction technique,” Mater. Sci. Tecnol., vol. 0836, 2017, doi: 10.1080/02670836.2016.1216027. [38] H. K. D. H. Bhadeshia, “Interpretation of the Microstructure of Steels,” https://www.phase-trans.msm.cam.ac.uk/. . [39] H. K. D. H. Bhadeshia, “Widmanstatten Ferrite,” https://www.phase-trans.msm.cam.ac.uk/. . [40] H. K. D. H. Bhadeshia and R. Honeycombe, “Related to carbide-free bainitic steels and method of producing such steels, US5879474A,” 2017. [41] G. I. Rees and H. K. D. H. Bhadeshia, “Bainite transformation kinetics Part 1 Modified model,” Mater. Sci. Technol., vol. 0836, 2013, doi: 10.1179/mst.1992.8.11.985. [42] S. B. Singh and H. K. D. H. Bhadeshia, “Estimation of bainite plate-thickness in low alloy steels,” Mater. Sci. Eng., 1997. [43] W. M. Johnson, “Reaction kinetics in processes of nucleation and growth,” Trans. Am. Inst. Min. Metall. Eng., vol. 135, pp. 419–442, 1939. [44] F. G. Caballero, H. K. D. H. Bhadeshia, K. J. a. Mawella, D. G. Jones, and P. Brown, “Design of novel high strength bainitic steels: Part 2,” Mater. Sci. Technol., vol. 17, no. 5, pp. 517–522, 2001, doi: 10.1179/026708301101510357. [45] D. V. Pereloma, E., & Edmonds, “Phase transformations in steels: Diffusionless transformations, high strength steels, modelling and advanced analytical techniques,” Elsevier, 2012. [46] H. K. D. H. Bhadeshia and V. Jerath, “Related to carbide-free bainitic steels and method of producing such steels,” 1996. [47] V. C. Igwemezie and P. C. Agu, “Development of Bainitic Steels for Engineering,” Int. J. Eng. Res. Tech, vol. 3, no. 2, pp. 2698–2711, 2014. [48] H. K. D. H. Bhadeshia., “Novel Steels for Rails,” in Encyclopedia of Materials Science: Science and Technology, 2002, pp. 1–7. [49] F. Fau et al., “Short note Subject : Stress corrosion testing of B360 bainitic and R260Mn pearlitic rails for Prorail,” no. 02280000, pp. 1–10, 2014. [50] H. M. Smith, “The characterization of ‘Carbide-Free’ bainitic rail steels in terms of their tempering, cold-working and rolling contact wear behaviour - British Steel- By private communication. no. S2286,” 1997. [51] H. M. Smith, L. J. Drewett, G. Thomson, V. Jerath, J. Jaiswal, and By private communication, “Bainitic Rail Steel Developments: A technical status report,” 2000. [52] L. Drewett, “Welding issues on Tata Steel bainitic rail steels. By private communication.,” 2014. [53] P. Secordel, “Review of B360 and B320- British Steel- By private communication,” 2019. [54] “Private communication by British Steel.” . [55] D. Tawfik, P. J. Mutton, and W. K. Chiu, “Experimental and numerical investigations: Alleviating tensile residual stresses in flash-butt welds by localised rapid post-weld heat treatment,” J. Mater. Process. Technol., vol. 196, no. 1–3, pp. 279–291, Jan. 2008, doi: 10.1016/J.JMATPROTEC.2007.05.055. [56] W. Li, G. Xiao, Z. Wen, X. Xiao, and X. Jin, “Plastic deformation of curved rail at rail weld caused by train – track dynamic interaction,” Wear, vol. 271, no. 1–2, pp. 311–318, 2011, doi: 10.1016/j.wear.2010.10.002. [57] G. Demofonti, S. Budano, and C. Viglialoro, “Role of residual stresses and microstructure on fatigue initiation and crack growth in welded rails. Office f. Official Publ. of the Europ. Communities.,” 1998. [58] “Flash butt welding technology for rails-a review . British Steel - By private communication,” 2008. [59] H. Farhangi and M. Engineering, “HORIZONTAL SPLIT-WEB FRACTURES OF FLASH BUTT,” no. November, pp. 509–517, 2007. [60] S. Gleeson, “Knowledge transfer session- British Steel - By private communication.” 2019. [61] P. R. VISHNU, Solid state transformations in weldments. 1993. [62] R. Lewis, Wheel-Rail Interface Handbook. 2009. [63] M. Pástor, “Introducción a la metalurgia de la soldadura.,” p. 350, 2005. [64] A. SAARNA, M; LAANSOM, “Rail and rail weld testing,” Proc. 4th Int. DAAAM Conf. Ind. Eng. as Compet. Edge SME, pp. 217–219, 2004. [65] “The influence of the working procedures on the formation and shape of the HAZ of flash butt and aluminothermic welds in rails . INNOTRACK. Project no. TIP5-CT-2006-031415,” 2008. [66] H. M. Smith, “Narrow HAZ B360 - Power Point presentation - British Steel - By private communication,” 2008. [67] BS EN 14587-1:2018. Railway applications. Infrastructure. Flash butt welding of new rails. R220, R260, R260Mn, R320Cr, R350HT, R350LHT, R370CrHT and R400HT grade rails in a fixed plant. [68] S. H. M. Boulanger D., Rouquie P., “Narrow HAZ B360 flash butt B360 welds - British Steel- By private communication,” 2006. [69] O. Engler and V. Randle, Introduction to texture analysis. 2010. [70] et al. CARTER, BARRY AUTOR, “Transmission Electron Microscopy: A Textbook for Materials Science,” Springer Sci. Bus. Media, vol. 1, 1996. [71] E1558-09, “Standard guide for eletrolytic polishing of metallographic specimens”ASTM Int. vol 09. 2019. [72] P. Secordel and H. Smith, “The development of a revised procedure for the flash butt welding of the B360 grade,” 2011. [73] H. M. Smith, “Development of a revised procedure for the FBW of a bainitic B360 rail - British Steel - By private communication,” 2011. [74] S. I. Kuchuk-Yatsenko, “Flash-butt welding of high-strength rails,” Mining–Informatics, Autom. Electr. Eng. 54, 2016. [75] X. Luo, X. Chen, T. Wang, S. Pan, and Z. Wang, “Effect of morphologies of martensite–austenite constituents on impact toughness in intercritically reheated coarse-grained heat-affected zone of HSLA steel,” Mater. Sci. Eng. A, vol. 710, no. October 2017, pp. 192–199, 2018 [76] M. T. Morito, S., Nishikawa, J., “Dislocation density within lath martenstie in Fe-C and Fe-Ni alloys,” vol. 43, no. 9, pp. 1475–1477, 2003. [77] M. Saarna and A. Laansoo, “Rail and rail weld testing,” no. April, 2004. [78] C. B. Huppi, G.S.; Damkroger, B.K.;Dallam, “Metallography and microstructures of weldments,” in ASM Handbook, Volume 9: Metallography and microstructures, 2004, pp. 1047–1056. [79] H. M. Smith, “A metallurgical examination of SBB Thermit welded grade 360 grooved Ri60 bainitic rails - British Steel - By private communication,” 2003. [80] H. M. Smith, “A metallurgical examination of an SBB flash butt welded 60E1 grade 360 bainitic rail - British Steel - By Private communication - n. 110586,” 2004. [81] S. H. Talebi, M. Jahazi, and H. Melkonyan, “Retained austenite decomposition and carbide precipitation during isothermal tempering of a medium-carbon low-alloy bainitic steel,” Materials (Basel)., vol. 11, no. 8, 2018 [82] Y. Ju, A. Goodall, M. Strangwood, and C. Davis, “Characterisation of precipitation and carbide coarsening in low carbon low alloy Q&T steels during the early stages of tempering,” Mater. Sci. Eng. A, vol. 738, no. August, pp. 174–189, 2018 [83] L. RYDE, “Application of EBSD to analysis of microstructures in commercial steels,” vol. 11, p. 1297,1306, 2006. [84] J. K. BOWLES, J.S.; MACKENZIE, “The crystallography of martensite transformations III. Face-centred cubic to bodu centred tretragonal transformations,” Acta Metall., vol. 2, no. 2, pp. 224–234. [85] P. Secordel, “Influence du Vanadium sur la resistance au revenu du B320 - British Steel, Hayange,” 2019. [86] H. M. Smith, “A metallurgical examination of a flash butt welded grade B360 60E1 rail for SBB - British Steel- By private communication. Project number: 1064719,” 2009. [87] H. A. Aglan, S. Ahmed, K. R. Prayakarao, and M. Fateh, “Effect of Preheating Temperature on the Mechanical and Fracture Properties of Welded Pearlitic Rail Steels,” Engineering, vol. 05, no. 11, pp. 837–843, 2013, doi: 10.4236/eng.2013.511101. [88] D. Tawfik, O. Kirstein, P. J. Mutton, and W. K. Chiu, “Verification of residual stresses in flash-butt-weld rails using neutron diffraction,” Phys. B Condens. Matter, vol. 385–386, pp. 894–896, 2006 [89] C. W. Ziemian, M. M. Sharma, and D. E. Whaley, “Effects of flashing and upset sequences on microstructure, hardness, and tensile properties of welded structural steel joints,” Mater. Des., vol. 33, no. 1, pp. 175–184, 2012 [90] H. M. Smith, “Development of bainitic rails for commercial track applications - British Steel- By private communication,” 2002. [91] Z. P. B. D. Popovic and H. P. Neff, “Introductory Electromagnetics,” Prentice Hall, no. April, pp. 1–581, 2000 [92] H. Mansouri and A. Monshi, “Microstructure and residual stress variations in weld zone of flash-butt welded railroads,” Sci. Technol. Weld. Join., vol. 9, no. 3, pp. 237–245, 2004 [93] D. C. Kim, W. J. So, and M. J. Kang, “Effect of flash butt welding parameters on weld quality of mooring chain,” Arch. Mater. Sci. Eng., vol. 38, no. 2, pp. 112–117, 2009. [94] W. Leonhard, K. Jörg, and E. Norbert, “Temperature Field Evolution During Flash Butt Welding of Railway Rails,” no. January, 2017 [95] Z. Xiong, S. Liu, X. Wang, C. Shang, X. Li, and R. D. K. Misra, “The contribution of intragranular acicular ferrite microstructural constituent on impact toughness and impeding crack initiation and propagation in the heat-affected zone (HAZ) of low-carbon steels,” Mater. Sci. Eng. A, vol. 636, pp. 117–123, 2015 [96] E. Mazancova, A. Jonsta, and E. Al, “Physical Metallurgy of Acicular Ferrite Formation,” Acta Metall. Slovaca, vol. 3, pp. 1–6, 2003. [97] O. P. Modi, N. Deshmukh, D. P. Mondal, A. K. Jha, A. H. Yegneswaran, and H. K. Khaira, “Effect of interlamellar spacing on the mechanical properties of 0.65% C steel,” Mater. Charact., vol. 46, no. 5, pp. 347–352, 2001 [98] H. A. Aglan, Z. Y. Liu, M. F. Hassan, and M. Fateh, “Mechanical and fracture behavior of bainitic rail steel,” J. Mater. Process. Technol., vol. 151, no. 1-3 SPEC. ISS., pp. 268–274, 2004 [99] S. Fretwell-smith, S. Danks, R. Lambert, R. Walker, and D. Benton, “Examination of a Mobile Flashbutt Weld produced at Crossrail - British Steel - By private communication. B700-20 R058,” 2016. [100] P. Secordel, “Bainitic rail presentation. Rail Annual Technical Forum 2019 - British Steel- By private communication,” 2020."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Eng.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/28596/1/Welding%20of%20carbide%20free%20bainitic%20steels%20for%20railway%20applications_%20final%20submission_MMM.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Carbide Free Bainitic (CFB) steels B360 and B320 show an outstanding behaviour in terms of fatigue deformation mechanisms, mainly when analysing its resistance to head checks. This, results in a lower necessity for maintenance and therefore, in a reduction of costs. However, problems have been encountered when welding CFB rails, showing cracks when in track, in both the entry and the exit site of the weld. The mechanisms of failure of these rails is not entirely clear. Nowadays, with the rise in use of high-speed trains and high loads, Continuously Welded Rails (CWR) are gaining importance; as other joining mechanisms such as fish-plates are becoming obsolete. Almost 90% of the CWR are welded by Flash Butt Welding (FBW); which is known as one of the most reliable welding processes; nevertheless, the welds are a weak link between rails due to mechanical and microstructural variations with the parent rail. Welding of conventional pearlitic rail steels, has been under investigation on numerous occasions; however, the same has not been made as extensively on CFB rail steels. On this thesis, an extensive examination of the Heat Affected Zone (HAZ) of three FBW rails (B360, B320 and R260) is discussed. CFB FBWs showed much wider HAZ extension than conventional pearlitic steels, of importance will be the extension of the tempered or Subcritical HAZ (SCHAZ), as CFBs, mainly B360 has shown low resistance to tempering; which could result on preferential wear and plastic deformation in track applications. With the purpose of reducing the extension of the tempered SCHAZ, weld trials were carried out on B360 rails using a stationary FBW GAAS 80 / 580 Schlatter welding machine in Scunthorpe, UK. Those, were produced by variations on the number of Pre-Heat (PH) cycles, on the preheating time (s) (ON) and delay period (s) (OFF) and additions of Post Weld Heat Pulses (PWHP) at the end of the welds. Finally, an analysis of the welded rails mechanical properties was made."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Welding of carbide-free bainitic steels for railway applications"]}]}],"canonical_facts":{"dc:contributor.advisor":["Palmiere, Eric J","Smith, Lindsey"],"dc:creator":["Muniz-Mangas, Marta"],"dc:date":["2021-03"],"dc:date.issued":["2021-03"],"dc:description.abstract":["Carbide Free Bainitic (CFB) steels B360 and B320 show an outstanding behaviour in terms of fatigue deformation mechanisms, mainly when analysing its resistance to head checks. This, results in a lower necessity for maintenance and therefore, in a reduction of costs. However, problems have been encountered when welding CFB rails, showing cracks when in track, in both the entry and the exit site of the weld. The mechanisms of failure of these rails is not entirely clear. Nowadays, with the rise in use of high-speed trains and high loads, Continuously Welded Rails (CWR) are gaining importance; as other joining mechanisms such as fish-plates are becoming obsolete. Almost 90% of the CWR are welded by Flash Butt Welding (FBW); which is known as one of the most reliable welding processes; nevertheless, the welds are a weak link between rails due to mechanical and microstructural variations with the parent rail. Welding of conventional pearlitic rail steels, has been under investigation on numerous occasions; however, the same has not been made as extensively on CFB rail steels. On this thesis, an extensive examination of the Heat Affected Zone (HAZ) of three FBW rails (B360, B320 and R260) is discussed. CFB FBWs showed much wider HAZ extension than conventional pearlitic steels, of importance will be the extension of the tempered or Subcritical HAZ (SCHAZ), as CFBs, mainly B360 has shown low resistance to tempering; which could result on preferential wear and plastic deformation in track applications. With the purpose of reducing the extension of the tempered SCHAZ, weld trials were carried out on B360 rails using a stationary FBW GAAS 80 / 580 Schlatter welding machine in Scunthorpe, UK. Those, were produced by variations on the number of Pre-Heat (PH) cycles, on the preheating time (s) (ON) and delay period (s) (OFF) and additions of Post Weld Heat Pulses (PWHP) at the end of the welds. Finally, an analysis of the welded rails mechanical properties was made."],"dc:format":["text"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/28596/1/Welding%20of%20carbide%20free%20bainitic%20steels%20for%20railway%20applications_%20final%20submission_MMM.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Faculty of Engineering (Sheffield)","Materials Science and Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/28596/"],"dc:relation.references":["[1] R. A. Smith, “Rolling Contact Fatigue of Rails: What Remains to be Done?,” China Railw. Serv., vol. 3, p. 001, 2002. [2] U. Zerbst, R. Lundén, K.-O. Edel, and R. A. Smith, “Introduction to the damage tolerance behaviour of railway rails – a review,” Eng. Fract. Mech., vol. 76, no. 17, pp. 2563–2601, Nov. 2009 [3] R. Sawley, K. & REIFF, “Rail failure assessment for the office of the rail regulator. An assessment of rail track’s methods for managing broken and defective rails. Report of the transportation Technology centre, Colorado, USA,” 2020. [4] H. Smith, “Bainitic rail steels- By private comunication- British Steel,” 2008. [5] V. A. Profidillis, Railway engineering. Brookfield, USA: Avebury Technical, 1995. [6] C. E. Volos, “Interaction between superstructure and substructure in railways,” Concrete, no. 5, pp. 2–9, 2010. [7] Chandra Satish and Agarwal M.M., “Railway Engineering (2nd Edition),” Oxford Univ. Press, vol. 20, pp. 1–2, 2015 [8] T. C. Abadi, “Effect of sleeper and ballast interventions on rail track performance,” University of Southampton, 2015. [9] S. Iwnicki, “Future trends in railway engineering,” Proc. Inst. Mech. Eng. Part C J. Mech. Eng. Sci., vol. 223, pp. 2743–2750, 2009 [10] D. Bilow and G. Randich, “Slab track for the next 100 years,” Am. Railw. Eng. Maintenance-of-w. Assoc. - Proc. 2000 Annu. Conf., no. 1, pp. 1–20, 2000. [11] Y. Bezin, D. Farrington, C. Penny, B. Temple, and S. Iwnicki, “The dynamic response of slab track constructions and their benefit with respect to conventional ballasted track,” Veh. Syst. Dyn., vol. 48, no. SUPPL. 1, pp. 175–193, 2010 [12] D. Campbell, J. Brougham, and R. Caldwell, “Uncovering and Understanding Australia’s First Railway,” Aust. J. Multi-Disciplinary Eng., vol. 7, no. 2, pp. 147–156, 2017 [13] J. Fernández, L. Museo, and D. Ferrocarril De Asturias, “Del Hierro Al Acero: La Producción De Duro Para La Compañía Del Noroeste Los Primeros Carriles Fabricados En España,” pp. 1–12, [14] R. I. Carroll, “Surface Metallurgy and Rolling Contact Fatigue of Rail,” University of Sheffield, 2005. [15] J. Locke, “The advent of the steel rail 1857-1914,” J. Transp. Hist., pp. 18–31, 1914. [16] A. S. J. A. Z. Jilabi, “Welding of Rail Steels,” University of Manchester, 2015. [17] P. Connor, “Track basics,” Railway Technical Website, no. 2, pp. 1–13. [18] EN13674-1 European standard UIC60/60E1 900A railway steel rail. . [19] U. Olofsson and T. Telliskivi, “Wear, plastic deformation and friction of two rail steels - A full-scale test and a laboratory study,” Wear, vol. 254, no. 1–2, pp. 80–93, 2003 [20] E. Sheinman, “Wear of rails. A review of the American press,” J. Frict. Wear, vol. 33, no. 4, pp. 308–314, 2012 [21] K. M. Lee and A. A. Polycarpou, “Wear of conventional pearlitic and improved bainitic rail steels,” Wear, vol. 259, no. 1–6, pp. 391–399, Jul. 2005 [22] S. Fretwell-smith, R. Steel, and D. Driver, “Rail Degradation Mechanisms - British Steel- By private communication,” 2012. [23] E. Magel, P. Sroba, K. Sawley, and J. Kalousek, “Control of rolling contact fatigue of rails,” Cent. Surf. Transp. Technol., pp. 1–29, 2005 [24] J. E. Garnham, D. I. Fletcher, C. L. Davis, and F. J. Franklin, “Visualization and modelling to understand rail rolling contact fatigue cracks in three dimensions,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 225, no. 2, pp. 165–178, 2011 [25] H. M. Smith, “Bainitic presentation February 2011- British Steel- By private communication.” 2011 . [26] T. Mount and H. Street, “Squats and squat-type defects in rails : the understanding to date,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, pp. 235–242, 2011 [27] L. J. Drewett, “The Measurement of Residual Stresses - British Steel- By private communication,” 2001. [28] H. Xiao, Q. Chen, E. Shao, D. Wu, Z. Chen, and Z. Wang, “The effect of shot peening on rolling contact fatigue behaviour and its crack initiation and propagation in carburized steel,” Wear, vol. 151, no. 1, pp. 77–86, 1991 [29] H. M. Smith, “The bainitic rail steel - Key property requirements - British Steel- By private communication,” 1998. [30] J. Jaiswal and C. Rail, “CORUS PREMIUM GRADES TO ADRESS WEAR - British Steel - By private communication.” [31] A. C. Athukorala, D. V. De Pellegrin, and K. I. Kourousis, “Characterisation of head-hardened rail steel in terms of cyclic plasticity response and microstructure for improved material modelling,” Wear, vol. 366–367, pp. 416–424, 2016 [32] H. K. D. H. Bhadeshia, “Bainite in Steels,” 2001. [33] J. Kalousek, D. M. Fegredo, and E. E. Laufer, “The wear resistance and worn metallography of pearlite, bainite and tempered martensite rail steel microstructures of high hardness,” Wear, vol. 105, pp. 199–222, 1985. [34] P. Clayton and N. Jin, “Unlubricated sliding and rolling/sliding wear behavior of continuously cooled, low/medium carbon bainitic steels,” Wear, vol. 200, no. 1–2, pp. 74–82, Dec. 1996 [35] H. K. D. H. Bhadeshia and D. V. Edmonds, “Bainite in silicon steels: new composition–property approach Part 1,” Met. Sci., vol. 17, no. September, pp. 420–425, 1983, doi: 10.1179/030634583790420646. [36] H. K. D. H. Bhadeshia, “Some phase transformations in steels,” Mater. Sci. Technol., vol. 0836, no. 1999, 2013 [37] Y. T. Chi, Y. T. Tsai, B. M. Huang, and J. R. Yang, “Investigation of idiomorphic ferrite and allotriomorphic ferrite using electron backscatter diffraction technique,” Mater. Sci. Tecnol., vol. 0836, 2017, doi: 10.1080/02670836.2016.1216027. [38] H. K. D. H. Bhadeshia, “Interpretation of the Microstructure of Steels,” https://www.phase-trans.msm.cam.ac.uk/. . [39] H. K. D. H. Bhadeshia, “Widmanstatten Ferrite,” https://www.phase-trans.msm.cam.ac.uk/. . [40] H. K. D. H. Bhadeshia and R. Honeycombe, “Related to carbide-free bainitic steels and method of producing such steels, US5879474A,” 2017. [41] G. I. Rees and H. K. D. H. Bhadeshia, “Bainite transformation kinetics Part 1 Modified model,” Mater. Sci. Technol., vol. 0836, 2013, doi: 10.1179/mst.1992.8.11.985. [42] S. B. Singh and H. K. D. H. Bhadeshia, “Estimation of bainite plate-thickness in low alloy steels,” Mater. Sci. Eng., 1997. [43] W. M. Johnson, “Reaction kinetics in processes of nucleation and growth,” Trans. Am. Inst. Min. Metall. Eng., vol. 135, pp. 419–442, 1939. [44] F. G. Caballero, H. K. D. H. Bhadeshia, K. J. a. Mawella, D. G. Jones, and P. Brown, “Design of novel high strength bainitic steels: Part 2,” Mater. Sci. Technol., vol. 17, no. 5, pp. 517–522, 2001, doi: 10.1179/026708301101510357. [45] D. V. Pereloma, E., & Edmonds, “Phase transformations in steels: Diffusionless transformations, high strength steels, modelling and advanced analytical techniques,” Elsevier, 2012. [46] H. K. D. H. Bhadeshia and V. Jerath, “Related to carbide-free bainitic steels and method of producing such steels,” 1996. [47] V. C. Igwemezie and P. C. Agu, “Development of Bainitic Steels for Engineering,” Int. J. Eng. Res. Tech, vol. 3, no. 2, pp. 2698–2711, 2014. [48] H. K. D. H. Bhadeshia., “Novel Steels for Rails,” in Encyclopedia of Materials Science: Science and Technology, 2002, pp. 1–7. [49] F. Fau et al., “Short note Subject : Stress corrosion testing of B360 bainitic and R260Mn pearlitic rails for Prorail,” no. 02280000, pp. 1–10, 2014. [50] H. M. Smith, “The characterization of ‘Carbide-Free’ bainitic rail steels in terms of their tempering, cold-working and rolling contact wear behaviour - British Steel- By private communication. no. S2286,” 1997. [51] H. M. Smith, L. J. Drewett, G. Thomson, V. Jerath, J. Jaiswal, and By private communication, “Bainitic Rail Steel Developments: A technical status report,” 2000. [52] L. Drewett, “Welding issues on Tata Steel bainitic rail steels. By private communication.,” 2014. [53] P. Secordel, “Review of B360 and B320- British Steel- By private communication,” 2019. [54] “Private communication by British Steel.” . [55] D. Tawfik, P. J. Mutton, and W. K. Chiu, “Experimental and numerical investigations: Alleviating tensile residual stresses in flash-butt welds by localised rapid post-weld heat treatment,” J. Mater. Process. Technol., vol. 196, no. 1–3, pp. 279–291, Jan. 2008, doi: 10.1016/J.JMATPROTEC.2007.05.055. [56] W. Li, G. Xiao, Z. Wen, X. Xiao, and X. Jin, “Plastic deformation of curved rail at rail weld caused by train – track dynamic interaction,” Wear, vol. 271, no. 1–2, pp. 311–318, 2011, doi: 10.1016/j.wear.2010.10.002. [57] G. Demofonti, S. Budano, and C. Viglialoro, “Role of residual stresses and microstructure on fatigue initiation and crack growth in welded rails. Office f. Official Publ. of the Europ. Communities.,” 1998. [58] “Flash butt welding technology for rails-a review . British Steel - By private communication,” 2008. [59] H. Farhangi and M. Engineering, “HORIZONTAL SPLIT-WEB FRACTURES OF FLASH BUTT,” no. November, pp. 509–517, 2007. [60] S. Gleeson, “Knowledge transfer session- British Steel - By private communication.” 2019. [61] P. R. VISHNU, Solid state transformations in weldments. 1993. [62] R. Lewis, Wheel-Rail Interface Handbook. 2009. [63] M. Pástor, “Introducción a la metalurgia de la soldadura.,” p. 350, 2005. [64] A. SAARNA, M; LAANSOM, “Rail and rail weld testing,” Proc. 4th Int. DAAAM Conf. Ind. Eng. as Compet. Edge SME, pp. 217–219, 2004. [65] “The influence of the working procedures on the formation and shape of the HAZ of flash butt and aluminothermic welds in rails . INNOTRACK. Project no. TIP5-CT-2006-031415,” 2008. [66] H. M. Smith, “Narrow HAZ B360 - Power Point presentation - British Steel - By private communication,” 2008. [67] BS EN 14587-1:2018. Railway applications. Infrastructure. Flash butt welding of new rails. R220, R260, R260Mn, R320Cr, R350HT, R350LHT, R370CrHT and R400HT grade rails in a fixed plant. [68] S. H. M. Boulanger D., Rouquie P., “Narrow HAZ B360 flash butt B360 welds - British Steel- By private communication,” 2006. [69] O. Engler and V. Randle, Introduction to texture analysis. 2010. [70] et al. CARTER, BARRY AUTOR, “Transmission Electron Microscopy: A Textbook for Materials Science,” Springer Sci. Bus. Media, vol. 1, 1996. [71] E1558-09, “Standard guide for eletrolytic polishing of metallographic specimens”ASTM Int. vol 09. 2019. [72] P. Secordel and H. Smith, “The development of a revised procedure for the flash butt welding of the B360 grade,” 2011. [73] H. M. Smith, “Development of a revised procedure for the FBW of a bainitic B360 rail - British Steel - By private communication,” 2011. [74] S. I. Kuchuk-Yatsenko, “Flash-butt welding of high-strength rails,” Mining–Informatics, Autom. Electr. Eng. 54, 2016. [75] X. Luo, X. Chen, T. Wang, S. Pan, and Z. Wang, “Effect of morphologies of martensite–austenite constituents on impact toughness in intercritically reheated coarse-grained heat-affected zone of HSLA steel,” Mater. Sci. Eng. A, vol. 710, no. October 2017, pp. 192–199, 2018 [76] M. T. Morito, S., Nishikawa, J., “Dislocation density within lath martenstie in Fe-C and Fe-Ni alloys,” vol. 43, no. 9, pp. 1475–1477, 2003. [77] M. Saarna and A. Laansoo, “Rail and rail weld testing,” no. April, 2004. [78] C. B. Huppi, G.S.; Damkroger, B.K.;Dallam, “Metallography and microstructures of weldments,” in ASM Handbook, Volume 9: Metallography and microstructures, 2004, pp. 1047–1056. [79] H. M. Smith, “A metallurgical examination of SBB Thermit welded grade 360 grooved Ri60 bainitic rails - British Steel - By private communication,” 2003. [80] H. M. Smith, “A metallurgical examination of an SBB flash butt welded 60E1 grade 360 bainitic rail - British Steel - By Private communication - n. 110586,” 2004. [81] S. H. Talebi, M. Jahazi, and H. Melkonyan, “Retained austenite decomposition and carbide precipitation during isothermal tempering of a medium-carbon low-alloy bainitic steel,” Materials (Basel)., vol. 11, no. 8, 2018 [82] Y. Ju, A. Goodall, M. Strangwood, and C. Davis, “Characterisation of precipitation and carbide coarsening in low carbon low alloy Q&T steels during the early stages of tempering,” Mater. Sci. Eng. A, vol. 738, no. August, pp. 174–189, 2018 [83] L. RYDE, “Application of EBSD to analysis of microstructures in commercial steels,” vol. 11, p. 1297,1306, 2006. [84] J. K. BOWLES, J.S.; MACKENZIE, “The crystallography of martensite transformations III. Face-centred cubic to bodu centred tretragonal transformations,” Acta Metall., vol. 2, no. 2, pp. 224–234. [85] P. Secordel, “Influence du Vanadium sur la resistance au revenu du B320 - British Steel, Hayange,” 2019. [86] H. M. Smith, “A metallurgical examination of a flash butt welded grade B360 60E1 rail for SBB - British Steel- By private communication. Project number: 1064719,” 2009. [87] H. A. Aglan, S. Ahmed, K. R. Prayakarao, and M. Fateh, “Effect of Preheating Temperature on the Mechanical and Fracture Properties of Welded Pearlitic Rail Steels,” Engineering, vol. 05, no. 11, pp. 837–843, 2013, doi: 10.4236/eng.2013.511101. [88] D. Tawfik, O. Kirstein, P. J. Mutton, and W. K. Chiu, “Verification of residual stresses in flash-butt-weld rails using neutron diffraction,” Phys. B Condens. Matter, vol. 385–386, pp. 894–896, 2006 [89] C. W. Ziemian, M. M. Sharma, and D. E. Whaley, “Effects of flashing and upset sequences on microstructure, hardness, and tensile properties of welded structural steel joints,” Mater. Des., vol. 33, no. 1, pp. 175–184, 2012 [90] H. M. Smith, “Development of bainitic rails for commercial track applications - British Steel- By private communication,” 2002. [91] Z. P. B. D. Popovic and H. P. Neff, “Introductory Electromagnetics,” Prentice Hall, no. April, pp. 1–581, 2000 [92] H. Mansouri and A. Monshi, “Microstructure and residual stress variations in weld zone of flash-butt welded railroads,” Sci. Technol. Weld. Join., vol. 9, no. 3, pp. 237–245, 2004 [93] D. C. Kim, W. J. So, and M. J. Kang, “Effect of flash butt welding parameters on weld quality of mooring chain,” Arch. Mater. Sci. Eng., vol. 38, no. 2, pp. 112–117, 2009. [94] W. Leonhard, K. Jörg, and E. Norbert, “Temperature Field Evolution During Flash Butt Welding of Railway Rails,” no. January, 2017 [95] Z. Xiong, S. Liu, X. Wang, C. Shang, X. Li, and R. D. K. Misra, “The contribution of intragranular acicular ferrite microstructural constituent on impact toughness and impeding crack initiation and propagation in the heat-affected zone (HAZ) of low-carbon steels,” Mater. Sci. Eng. A, vol. 636, pp. 117–123, 2015 [96] E. Mazancova, A. Jonsta, and E. Al, “Physical Metallurgy of Acicular Ferrite Formation,” Acta Metall. Slovaca, vol. 3, pp. 1–6, 2003. [97] O. P. Modi, N. Deshmukh, D. P. Mondal, A. K. Jha, A. H. Yegneswaran, and H. K. Khaira, “Effect of interlamellar spacing on the mechanical properties of 0.65% C steel,” Mater. Charact., vol. 46, no. 5, pp. 347–352, 2001 [98] H. A. Aglan, Z. Y. Liu, M. F. Hassan, and M. Fateh, “Mechanical and fracture behavior of bainitic rail steel,” J. Mater. Process. Technol., vol. 151, no. 1-3 SPEC. ISS., pp. 268–274, 2004 [99] S. Fretwell-smith, S. Danks, R. Lambert, R. Walker, and D. Benton, “Examination of a Mobile Flashbutt Weld produced at Crossrail - British Steel - By private communication. B700-20 R058,” 2016. [100] P. Secordel, “Bainitic rail presentation. Rail Annual Technical Forum 2019 - British Steel- By private communication,” 2020."],"dcterms:accessrights":["public"],"dc:title":["Welding of carbide-free bainitic steels for railway applications"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Eng.D"]},"updated_at":"2026-11-18T22:41:49Z"}