{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:28616"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:28616","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Micro-CT Scanning in the Investigation of Squat Defects in Rail Steel","abstract":"This thesis contains the results from an investigation into Squats, a discrete rail steel defect. Micro-computed tomography (micro-CT) scanning was used to scan the entire structure of four out of five defects removed from railway track. The fifth was not scanned as it shelled in track. The difficulty turning these raw X-ray images into a segmented 3D model were overcome by developing a new technique. Isolating separate regions of the scans created areas where voxel value variation was at a minimum (i.e. the histogram became one narrow peak rather than multiple broad peaks). This allowed the automatic crack segregation module to work fairly well, and then enhanced using the region growing modules within the software. These scan results were then verified to be accurate using metallographic sample preparation, optical and electron microscopy. Micro CT scanning was performed on a custom 450KeV scanner, allowing the capture of the first entire Squat crack network morphology. Full defect imaging allowed the different defects to be compared to each other, highlighting differences and similarities. The defects came from metro, mixed and high-speed railways and one was found within an aluminothermic weld. The verification process and investigations of the scan volumes yielded further information about the defect’s origins. These origins were used to determine that, for the five defects investigated, there were four different causes. The two that shared a cause were from the same track section. Based on the causes, the defects were identified as a Stud, two Grinding Induced Squats (GIS), a Squat (caused by the legacy issue of MnS inclusions) and possibly a Squat or Stud in a slightly contaminated weld. None of the defects were considered to be a classic Squat, which is caused by Rolling Contact Fatigue (RCF), because there were other factors in their initiation. One of the defects contained a transverse defect, which is a crack that grows down through the railhead and can break the rail. This transverse defect was ~9mm deep into the rail when it was removed, meaning it would not have returned to the surface to shell. A high-resolution volume of the transverse defect region was created and its origin gives an important insight into the potential causes of rail-breaking defects. The origin of this transverse defect was a cluster of debris-filled voids that had formed due to the corrosion and cyclic loading (fretting) of a crack branch. These voids aligned with a deep grinding mark on the surface of the rail, which acted as a stress raiser. Because corrosion is a factor in this transverse defect case, the age of a rail and its environment are factors for defect development as well as traffic volume, given the correlation of corrosion with time. Results of this work highlight both the importance of a good surface finish and the diversity of causes found within the term “Squat”. Thus the identification of the Stud variant may be the beginning of a more comprehensive group of Squat type defects being established. This refining of the category could lead to fruitful big data analyses of the Squat type defect occurrences. The CT volumes of the defects created in this work can easily be stored for comparison in future investigations. The virtual nature of the volumes allows the sharing of defect information more readily than physical and sectioned defects, which deteriorate with time and require physical storage and transport.","abstract_html":"This thesis contains the results from an investigation into Squats, a discrete rail steel defect. Micro-computed tomography (micro-CT) scanning was used to scan the entire structure of four out of five defects removed from railway track. The fifth was not scanned as it shelled in track. The difficulty turning these raw X-ray images into a segmented 3D model were overcome by developing a new technique. Isolating separate regions of the scans created areas where voxel value variation was at a minimum (i.e. the histogram became one narrow peak rather than multiple broad peaks). This allowed the automatic crack segregation module to work fairly well, and then enhanced using the region growing modules within the software. These scan results were then verified to be accurate using metallographic sample preparation, optical and electron microscopy. Micro CT scanning was performed on a custom 450KeV scanner, allowing the capture of the first entire Squat crack network morphology. Full defect imaging allowed the different defects to be compared to each other, highlighting differences and similarities. The defects came from metro, mixed and high-speed railways and one was found within an aluminothermic weld. The verification process and investigations of the scan volumes yielded further information about the defect’s origins. These origins were used to determine that, for the five defects investigated, there were four different causes. The two that shared a cause were from the same track section. Based on the causes, the defects were identified as a Stud, two Grinding Induced Squats (GIS), a Squat (caused by the legacy issue of MnS inclusions) and possibly a Squat or Stud in a slightly contaminated weld. None of the defects were considered to be a classic Squat, which is caused by Rolling Contact Fatigue (RCF), because there were other factors in their initiation. One of the defects contained a transverse defect, which is a crack that grows down through the railhead and can break the rail. This transverse defect was ~9mm deep into the rail when it was removed, meaning it would not have returned to the surface to shell. A high-resolution volume of the transverse defect region was created and its origin gives an important insight into the potential causes of rail-breaking defects. The origin of this transverse defect was a cluster of debris-filled voids that had formed due to the corrosion and cyclic loading (fretting) of a crack branch. These voids aligned with a deep grinding mark on the surface of the rail, which acted as a stress raiser. Because corrosion is a factor in this transverse defect case, the age of a rail and its environment are factors for defect development as well as traffic volume, given the correlation of corrosion with time. Results of this work highlight both the importance of a good surface finish and the diversity of causes found within the term “Squat”. Thus the identification of the Stud variant may be the beginning of a more comprehensive group of Squat type defects being established. This refining of the category could lead to fruitful big data analyses of the Squat type defect occurrences. The CT volumes of the defects created in this work can easily be stored for comparison in future investigations. The virtual nature of the volumes allows the sharing of defect information more readily than physical and sectioned defects, which deteriorate with time and require physical storage and transport.","abstract_has_math":false,"creators":["Earl, Shaun"],"institution":"University of Sheffield","degree_name":"Eng.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Rainforth, W. Mark","Lewis, Roger","Smith, Lindsey"],"committee_chairs":[],"committee_members":[],"year":2021,"date_issued":"2021-01","date_published":"2021-01","updated_at":"2026-11-18T22:41:49Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.826851"],"render_values":[{"text":"uk.bl.ethos.826851","href":null,"code":true}]},{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["EP/L016273/1 for hte CDT AMS"],"render_values":[{"text":"EP/L016273/1 for hte CDT AMS","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/28616/1/Shaun%20Earl%20Squats%20Thesis%20resubmission%20Jan%202021.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A28616","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Rainforth, W. Mark","Lewis, Roger","Smith, Lindsey"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["ESPRC"]},{"key":"dc:creator","label":"Author","values":["Earl, Shaun"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2021-01"]},{"key":"dc:date.issued","label":"Date","values":["2021-01"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Materials Science and Engineering (Sheffield)","Mechanical Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/28616/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["1.4 References [1] Network Rail, “Rail Head Squats,” 2015. [Online]. Available: https://cdn.networkrail.co.uk/wp-content/uploads/2017/03/Challenge-Statement-Track-Plain-line-rail-head-squats.pdf. [Accessed: 13-Jun-2018]. [2] E. N. Landis and D. T. Keane, “X-ray microtomography,” Mater. Charact., vol. 61, no. 12, pp. 1305–1316, 2010. [3] C. Jessop, J. Ahlström, L. Hammar, S. Fæster, and H. K. Danielsen, “3D characterization of rolling contact fatigue crack networks,” Wear, vol. 366–367, pp. 392–400, 2016. [4] M. Naeimi et al., “Reconstruction of the rolling contact fatigue cracks in rails using X-ray computed tomography,” NDT E Int., vol. 92, no. April, pp. 199–212, 2017. [5] J. J. Kalker, Three-dimensional elastic bodies in rolling contact. Kluwer Academic Publishers, 1990. [6] B. L. Singh and C. B. E. Sr, “Rolling Contact Fatigue in Rails – an Overview,” 2008. [Online]. Available: http://www.iricen.gov.in/iricen/ipwe_seminar/2011/paper_2_lalloosingh.pdf. [Accessed: 17-Jul-2020]. [7] W. Daniel, S. Pal, and M. . Farjoo, “Rail squats: progress in understanding the Australian experience,” J. Rail Rapid Transit, vol. 227, no. 5, pp. 481–492, 2013. [8] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. 2.9 References [1] Network Rail, “Rail Head Squats,” 2015. [Online]. Available: https://cdn.networkrail.co.uk/wp-content/uploads/2017/03/Challenge-Statement-Track-Plain-line-rail-head-Squats.pdf. [Accessed: 13-Jun-2018]. [2] K. L. Johnson, Contact Mechanics. Cambridge University Press, 1985. [3] H. Wu and N. Wilson, “Flange climb derailments: causes and prevention,” Int. Railw. J., vol. 52, no. 3, p. 47, 2012. [4] D. I. Fletcher and J. Beynon, “Development of a Machine for Closely Controlled Rolling Contact Fatigue and Wear Testing.,” J. Test. Eval., vol. 28, no. 4, p. 267, 2000. [5] R. S. Dwyer-Joyce, C. Yao, and R. Lewis, “A Comparison of Three Methods for the Measurement of Wheel Rail Contact,” STLE/ASME 2008 Int. Jt. Tribol. Conf., no. November 2015, pp. 541–543, 2008. [6] J. J. Kalker, Three-dimensional elastic bodies in rolling contact. Kluwer Academic Publishers, 1990. [7] J. J. Kalker, “A fast algorithm for the simplified theory of rolling contact,” Veh. Syst. Dyn., vol. 11, no. 1, 1982. [8] J. Srivastava, P. Sarkar, and V. Ranjan, “A numerical study on effects of friction-induced thermal load for rail under varied wheel slip conditions,” Simul. Trans. ofthe Soc. Model. Simul. Int., pp. 1–12, July 2018. [9] T. Telliskivi and U. Olofsson, “Contact mechanics analysis of measured wheel-rail profiles using the finite element method,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 215, no. 2, pp. 65–72, 2001. [10] A. Kapoor, F. J. Franklin, S. K. Wong, and M. Ishida, “Surface roughness and plastic flow in rail wheel contact,” vol. 253, pp. 257–264, 2002. [11] F. J. Franklin, I. Widiyarta, and A. Kapoor, “Computer simulation of wear and rolling contact fatigue,” Wear, vol. 250-251, pp. 949–955, 2001. [12] O. Arias-Cuevas, Z. Li, R. Lewis, and E. A. Gallardo-Hernández, “Rolling-sliding laboratory tests of friction modifiers in dry and wet wheel-rail contacts,” Wear, vol. 268, no. 3–4, pp. 543–551, 2010. [13] J. H. Al-Bedhany and H. Long, “Microscopic investigation of subsurface initiated damage of wind turbine gearbox bearings,” J. Phys. Conf. Ser., vol. 1106, no. 1, p.12029, 2018. [14] E. Magel and J. Kalousek, “Martensite and Contact Fatigue Initiated Wheel Defects,” in 12th International Wheelset Congress, 1998, pp. 100–111. [15] J. A. Williams, “The influence of repeated loading , residual stresses and shakedown on the behaviour of tribological contacts,” vol. 38, pp. 786–797, 2005. [16] E. Magel, “Rolling Contact Fatigue: A Comprehensive Review,” ECS Trans., vol. 28, no. 32, pp. 35–44, 2010. [17] S. R. Lewis, R. Lewis, and D. I. Fletcher, “Assessment of laser cladding as an option for repairing/enhancing rails,” Wear, vol. 330–331, no. July, pp. 581–591, 2015. [18] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [19] F. . Carter, “On the Action of a Locomotive Driving Wheel,” Proc. R. Soc., vol. A112, pp. 151–157, 1926. [20] J. J. Kalker, “Wheel — rail rolling contact theory,” vol. 144, pp. 243–261, 1991. [21] L. Smith, “Rolling Contact Fatigue in Wheel-Rail Contact,” University of Newcastle Upon Tyne, 2007. [22] R. Lewis and U. Olofsson, “Chapter 5: Tribology of the Wheel–Rail Contact,” in Handbook of Railway Vehicle Dynamics, S. Iwnicki, M. Spiryagin, C. Cole, and T. McSweeney, Eds. Taylor & Francis Group, LLC, 2006, p. 131. [23] R. Stock, L. Stanlake, C. Hardwick, M. Yu, D. Eadie, and R. Lewis, “Material concepts for top of rail friction management – Classification, characterisation and application,” Wear, vol. 366–367, pp. 225–232, 2016. [24] R. Stock, D. T. Eadie, D. Elvidge, and K. Oldknow, “Influencing rolling contact fatigue through top of rail friction modifier application - A full scale wheel-rail test rig Study,” Wear, vol. 271, no. 1–2, pp. 134–142, 2011. [25] J. Williams, Rolling contacts and rolling-element bearings. Cambridge University Press. [26] D. I. Fletcher and J. Beynon, “The effect of intermittent lubrication on the fatigue life of pearlitic rail steel in rolling- sliding contact,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 214, pp. 145–158, 2000. [27] M. Kaneta, K. Matsudo, K. Murakami, and H. Nishikawa, “1998 ASME Kaneta A Possible Mechanism.pdf,” ASME, vol. 120, pp. 304–309, 1998. [28] S. Bogda, P. Lewicki, and M. Szymaniak, “Experimental and theoretical investigation of the phenomenon of filling the RCF crack with liquid,” vol. 258, pp. 1280–1287, 2005. [29] N. Gao, R. S. Dwyer-Joyce, and D. G. G. Grieve, “Disc machine testing to assess the life of surface-damaged railway track,” Proc. Inst. Mech. Eng. Part F-Journal Rail Rapid Transit, vol. 215, no. 4, pp. 261–275, 2001. [30] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [31] C. Hardwick, R. Lewis, and R. Stock, “The effects of friction management materials on rail with pre existing rcf surface damage,” Wear, vol. 384–385, no. November 2016, pp. 50–60, 2017. [32] M. Sol-Sánchez, F. Moreno-Navarro, and M. C. Rubio-Gámez, “Analysis of ballast tamping and stone-blowing processes on railway track behaviour: the influence of using USPs,” Géotechnique, vol. 66, no. 6, pp. 481–489, 2016. [33] E. T. (Ernest T. Selig and J. M. Waters, Track geotechnology and substructure management. Thomas Telford, 1994. [34] J. Miss, “Running Surface Features and Defect Catalogue,” pp. 1-71, 2010. [35] NSW Transport RailCorp, “Rail Defects Handbook: TMC 226,” pp. 1–83, 2012. [36] P. Mutton, J. Cookson, C. Qiu, and D. Welsby, “Microstructural characterisation of rolling contact fatigue damage in flashbutt welds,” Wear, vol. 366–367, pp. 368–377, 2016. [37] E. Magel, M. Roney, J. Kalousek, and P. Sroba, “The blending of theory and practice in modern rail grinding,” Fatigue Fract. Eng. Mater. Struct., vol. 26, no. 10, pp. 921–929, 2003. [38] Bhadeshia, Harshad K. D. H., et al. Steels: Microstructure and Properties, Elsevier Science & Technology, 2006. [39] D. Aliya and A. Analytical, “Physical Metallurgy Concepts in Interpretation of Microstructures,” Metallogr. Microstruct., vol. 9, pp. 44–70, 2018. [40] University of Cambridge, “Interpretation of cooling curves.” [Online]. Available: https://www.doitpoms.ac.uk/tlplib/phase-diagrams/cooling.php. [Accessed: 29-Apr-2019]. [41] F. P. L. Kavishe and T. J. Baker, “Effect of prior austenite grain size and pearlite interlamellar spacing on strength and fracture toughness of a eutectoid rail steel,” Mater. Sci. Technol., vol. 2, no. 8, pp. 816–822, 2014. [42] H. W. Zhang, S. Ohsaki, S. Mitao, M. Ohnuma, and K. Hono, “Microstructural investigation of white etching layer on pearlite steel rail,” Mater. Sci. Eng. A, vol. 421, no. 1–2, pp. 191–199, 2006. [43] G. E. Totten and G. E. Totten, “Failures Related to Heat Treating Operations,” Fail. Anal. Prev., vol. 11, pp. 192–223, 2018. [44] International Union of Railways, “INNOTRACK concluding technical report,” Paris, France, 2010. [45] ARTC, “Rail Defects Handbook Some Rail Defects , their Characteristics , Causes and Control RC 2400,” no. March, 2006. [46] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. [47] V. Dikshit, P. Clayton, and D. Christensen, “Investigation of rolling contact fatigue in a head-hardened rail,” Wear, vol. 144, no. 1–2, pp. 89–102, 1991. [48] TataSteel, “Review of anti Squat research,” 2013. [49] R. Stock and R. Pippan, “Rail grade dependent damage behaviour – Characteristics and damage formation hypothesis,” Wear, vol. 314, no. 1–2, pp. 44–50, 2014. [50] W. Solano-Alvarez and H. K. D. H. Bhadeshia, “White-etching matter in bearing steel. Part I: Controlled cracking of 52100 steel,” Metall. Mater. Trans. A Phys. Metall. Mater. Sci., vol. 45, no. 11, pp. 4907–4915, 2014. [51] P. Clayton and M. B. P. Allery, “Metallurgical Aspects of Surface Damage Problems in Rails,” Can. Metall. Q., vol. 21, no. 1, pp. 31–46, 1982. [52] UIC, “Recommendations for the use of rail steel grades,” pp. 4, 2015. [53] E. Magel, P. Sroba, K. Sawley, and J. Kalousek, “Control of Rolling Contact Fatigue of Rails,”, pp. 8, 2005. [54] J. E. Garnham and C. L. Davis, “Very early stage rolling contact fatigue crack growth in pearlitic rail steels,” Wear, vol. 271, no. 1–2, pp. 100–112, 2011. [55] M. Burstow, “Experience of premium grade rail steels to resist rolling contact fatigue (RCF) on GB network,” Ironmak. Steelmak., vol. 40, no. 2, pp. 103–107, 2013. [56] A. D. Hearle and K. L. Johnson, “Mode II stress intensity factors for a crack parallel to the surface of an elastic half-space subjected to a moving point load,” J. Mech. Phys. Solids, vol. 33, no. 1, pp. 61–81, Jan. 1985. [57] A. Kapoor, D. I. Fletcher, and F. J. Franklin, “The role of wear in enhancing rail life,” Tribol. Ser., no. 41, pp. 331–340, 2002. [58] J. E. Garnham and J. Beynon, “The early detection of rolling-sliding contact fatigue cracks,” Wear, vol. 144, no. 1–2, pp. 103–116, 1991. [59] D. I. Fletcher, P. Hyde, and A. Kapoor, “Investigating fluid penetration of rolling contact fatigue cracks in rails using a newly developed full-scale test facility,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 221, pp. 35–44, 2007. [60] A. J. Perez-Unzueta and J. H. Beynon, “Microstructure and wear resistance of pearlitic rail steels.pdf,” Wear, vol. 162–164, pp. 173–82, 1993. [61] P. Clayton, “Tribological aspects of wheel-rail contact: a review of recent experimental research,” Wear, vol. 191, pp. 170–183, 1996. [62] J. F. Archard and W. Hirst, “The wear of metals under unlubricated conditions,” Proc. R. Soc. London., vol. 236, no. Ser. A. Math. Phys. Sci., pp. 397–410, 1956. [63] D. F. Cannon, K. O. Edel, S. L. Grassie, and K. Sawley, “Rail defects: An overview,” Fatigue Fract. Eng. Mater. Struct., vol. 26, no. 10, pp. 865–886, 2003. [64] S. B. Newcomb and W. M. Stobbs, “A transmission electron microscope Study of the white etching layer on a rail head,” Mater. Sci. Eng. A, vol. 66, pp. 195–204, 1984. [65] J. Wu, R. H. Petrov, M. Naeimi, Z. Li, R. Dollevoet, and J. Sietsma, “Laboratory simulation of martensite formation of white etching layer in rail steel,” Int. J. Fatigue, vol. 91, pp. 11–20, 2016. [66] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part I : Origination,” vol. 47, pp. 361–372, 2013. [67] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [68] S. Simon. De la dynamique ferroviaire `a l’accommodation microstructurale du rail : Contribution des TTS `a la r´eponse tribologique des aciers : Cas du d´efaut de squat. Mechanics of the solides. INSA de Lyon, 2014. French. [69] A. Al-juboori et al., “Squat formation and the occurrence of two distinct classes of white etching layer on the surface of rail steel,” vol. 104, pp. 52–60, 2017. [70] W. Lojkowski, M. Djahanbakhsh, G. Bürkle, S. Gierlotka, W. Zielinski, and H. J. Fecht, “Nanostructure formation on the surface of railway tracks,” Mater. Sci. Eng. A, vol. 303, no. 1–2, pp. 197–208, 2001. [71] S. Simon, A. Saulot, C. Dayot, X. Quost, and Y. Berthier, “Tribological characterization of rail Squat defects,” Wear, vol. 297, no. 1–2, pp. 926–942, 2013. [72] R. I. Carroll, “Surface Metallurgy and Rolling Contact Fatigue of Rail,” University of Sheffield, 2005. [73] F. Alwahdi, “Wear and Rolling Contact Fatigue of Ductile Materials,” University of Sheffield, 2004. [74] A. Ekberg, “D3.1- Enhanced track structure- Status, key influencing parameters and prioritised areas of improvement v.6,” pp. 11-12, 2018. [75] S. Li, J. Wu, R. H. Petrov, Z. Li, R. Dollevoet, and J. Sietsma, “‘Brown etching layer’: A possible new insight into the crack initiation of rolling contact fatigue in rail steels?,” Eng. Fail. Anal., vol. 66, pp. 8–18, 2016. [76] M. Steenbergen, “Squat formation and rolling contact fatigue in curved rail track,” Eng. Fract. Mech., vol. 143, pp. 80–96, 2015. [77] S. L. Grassie, “Rail corrugation: characteristics, causes, and treatments,” Proc. IMechE Vol. 223 Part F J. Rail Rapid Transit, pp. 581–596, 2009. [78] K. Kondo, K. Yoroizaka, and Y. Sato, “Cause, increase, diagnosis, countermeasures and elimination of Shinkansen shelling,” Wear, vol. 191, no. 1–2, pp. 99–203, 1996. [79] F. Fau, H. Smith, S. Fretwell-Smith, L. Deng, “Effect of grinding quality, lubri- cation quality and rail hardness on flaking defect initiation on high rails” Proceedings of the 10th International Conference on Contact Mechanics and Wear of Rail/Wheel Systems (CM2015), Colorado, USA, 30 August–3 September. [80] M. Steenbergen, “Rolling contact fatigue in relation to rail grinding,” Wear, vol. 356–357, pp. 110–121, 2016. [81] A. C. Athukorala, “Investigation of Wear and Ratcheting Response of Head-Hardened Australian Rail Steel under Conditions of Rolling Contact Fatigue,” Queensland University of Technology SCIENCE, 2016. [82] S. L. Grassie, “Squats and Squat-type defects in rails: the understanding to date,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 235–242, 2012. [83] S. L. Grassie, “Studs and Squats: The evolving story,” Wear, vol. 366–367, pp. 194–199, 2016. [84] M. Ishida, “Rolling contact fatigue (RCF) defects of rails in Japanese railways and its mitigation strategies,” Electron. J. Struct. Eng., vol. 13, no. 1, pp. 67–74, 2013. [85] S. L. Grassie, “Rolling contact fatigue on the British railway system : treatment,” vol. 258, no. June 2003, pp. 1310–1318, 2005. [86] Railtrack plc, Rolling contact fatigue in rails: a guide to current understanding and practice. Heron Press, Birmingham, UK, 2001. [87] M. Kerr, A. Wilson, and S. Marich, “The epidemiology of Squats and related rail defects,” CORE 2008 Conf. Railw. Eng. rail- the-core Integr. Transp., no. September, pp. 83–96, 2008. [88] S. Kaewunruen, M. Ishida. In Situ Monitoring of Rail Squats in Three Dimensions Using Ultrasonic Technique. Exp Tech 40, 1179–1185 (2016). [89] X. Zhao, Dynamic Wheel/Rail Rolling Contact at Singular Defects with Application on Squats. Southwest Jiaotong University, 2012. [90] M. Ishida, M. Akama, K. Kashiwaya, and A. Kapoor, “The current status of theory and practice on rail integrity in Japanese railways-rolling contact fatigue and corrugations,” Fatigue Fract. Eng. Mater. Struct., vol. 26, no. 10, pp. 909–919, 2003. [91] S. Kaewunruen, “Identification and prioritization of rail Squat defects in the field using rail magnetisation technology,” Struct. Heal. Monit. Insp. Adv. Mater. Aerospace, Civ. Infrastruct. 2015, vol. 9437, no. April 2015, p. 94371H, 2015. [92] S. Kaewunruen and M. Ishida, “Rail Squats: understand its causes, severity , and non-destructive evaluation techniques,” Proceedings of the 20th National Convention on Civil Engineering Vol. 1 Iss. 1, 2015. [93] Z. Li, X. Zhao, C. Esveld, R. Dollevoet, and M. Molodova, “An investigation into the causes of Squats-Correlation analysis and numerical modeling,” Wear, vol. 265, no. 9–10, pp. 1349–1355, 2008. [94] M. Kerr and W. Daniel, “Final Report on the Rail Squat Project R3-105,” CRC for Rail Innovation, Brisbane, 2011. [95] L. Deng, “Understanding of rail Squats from the point of view of metallurgy, Tata Steel internal presentation.” . [96] Z. Li, “Squats on Railway Rails,” in Wheel-Rail Interface Handbook, R. Lewis and U. Olofsson, Eds. Woodhead Publishing Limited, 2009. [97] E. Magel, P. Mutton, A. Ekberg, and A. Kapoor, “Rolling contact fatigue, wear and broken rail derailments,” Wear, vol. 366–367, pp. 249–257, 2016. [98] C. J. Rasmussen, X. Zhang, H. K. Danielsen, and S. Fæster, “Grinding induced martensite on the surface of rails,” Proc. 35th Risø Int. Symp. Mater. Sci. New Front. Nanometals, vol. 35, pp. 439–446, 2014. [99] M. Farjoo, W. Daniel, P. Bellette, and P. A. Meehan, “Field statistical and finite element analysis of rail Squats,” Eng. Fract. Mech., vol. 109, pp. 117–129, 2013. [100] Z. Li, R. Dollevoet, M. Molodova, and X. Zhao, “Squat growth — Some observations and the validation of numerical predictions,” Wear, vol. 271, no. 1–2, pp. 148–157, 2011. [101] M. Naeimi et al., “Reconstruction of the rolling contact fatigue cracks in rails using X-ray computed tomography,” NDT E Int., vol. 92, no. April, pp. 199–212, 2017. [102] C. Jessop, J. Ahlström, L. Hammar, S. Fæster, and H. K. Danielsen, “3D characterization of rolling contact fatigue crack networks,” Wear, vol. 366–367, pp. 392–400, 2016. [103] N. Gao, R. S. Dwyer-Joyce, and D. G. G. Grieve, “Disc machine testing to assess the life of surface-damaged railway track,” Proc. Inst. Mech. Eng. Part F-Journal Rail Rapid Transit, vol. 215, no. 4, pp. 261–275, 2001. [104] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part II : Growth,” vol. 47, pp. 373–381, 2013. [105] D. I. Fletcher and S. H. Sanusi, “the Potential for Supressing Rail Defect Growth Through Tailoring Rail Thermo-Mechanical Properties,” in 10th International Conference on Contact Mechanics and Wear of Rail/ Wheel System, 2015. [106] D. Scott, D. I. Fletcher, and B. J. Cardwell, “Simulation Study of Thermally Initiated Rail Defects,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 228, no. 2, pp. 113–127, 2012. [107] M. Kerr and A. Wilson, “Rail Squat Defects,” Perm. W. Inst. Inc, pp. 13–25, 2000. [108] Sperry Rail Service, “Rail Defect Manual,” p. 43, 1968. [109] Federal Railroad Administration, “Track Inspector Rail Defect Reference Manual,” 2015. [110] H. M. Smith, “An examination of Squat defects in a 60E1 R260 rail removed from the Bussy Saint Georges test site in the Paris suburbs ( RER line ),” Rotherham, UK, 2011. [111] M. Itabashi and K. Kawata, “Carbon content effect on high-strain-rate tensile properties for carbon steels,” Int. J. Impact Eng., vol. 24, no. 2, pp. 117–131, 2000. [112] Z. Popovic Radovic, V., “Analysis of cracking on running surface of rails,” Gradevinar, vol. 65, no. 3, pp. 251–259, 2013. [113] T. Szugs et al., “Combination of Ultrasonic and Eddy Current Testing with Imaging for Characterization of Rolling Contact Fatigue,” 19th World Conference on Non-Destructive Testing (WCNDT 2016), 13-17 June 2016 in Munich, Germany (WCNDT), 2016. [114] D. Peng and R. Jones, “Lock-in thermographic inspection of Squats on rail steel head,” Infrared Phys. Technol., vol. 57, pp. 89–95, 2013. [115] M. Molodova, Z. Li, A. Nunez, and R. Dollevoet, “Automatic Detection of Squats in Railway Infrastructure,” IEEE Traansactions Intell. Transp. Syst., vol. 15, no. 1, pp. 1980–1990, 2014. [116] Network Rail, “Re-Profiling Rail to Remove Defects & Extend Rail Life.” [Online]. Available: https://www.networkrail.co.uk/wp-content/uploads/2019/06/Challenge-statement-track-re-profiling-rail-to-remove-defects-and-extend-rail-life.pdf. [Accessed: 19-Aug-2019]. [117] Taubert, M. “High-speed grinding.” International Railway Journal, 45(12), p.40-41, 2005. [118] Network Rail, “Innovative, new grinding trains will help passenger and freight trains run smoothly and safely for years to come.” [Online]. Available: https://www.networkrailmediacentre.co.uk/news/innovative-new-grinding-trains-will-help-passenger-and-freight-trains-run-smoothly-and-safely-for-years-to-come. [Accessed: 09-Aug-2019]. [119] A. Faley, “Repair of a ‘Squat’ defect by thermit welding,” no. 919, pp. 95–97, 1979. 3.6 References [1] A. H. Compton and D. Ph, “THE SCATTERING OF X-RAYS TIIE present paper will be confined to a discussion of some of the points which present to us a revolutionary change in our ideas regarding the process of scattering of electromagnetic waves . No attempt will be made to describe t,” vol. 198, no. 1183, 1923. [2] Iowa State University NDT Education Resource Centre, “Sources of Attenuation,” 2014. [Online]. Available: https://www.nde-ed.org/EducationResources/CommunityCollege/Radiography/Physics/attenuation.htm. [Accessed: 07-Jul-2019]. [3] H. Chen, M. M. Rogalski, and J. N. Anker, “Advances in functional X-ray imaging techniques and contrast agents,” Phys. Chem. Chem. Phys., vol. 14, no. 39, pp. 13469–13486, 2012. [4] R. Nave, “X-ray production.” [Online]. Available: http://hyperphysics.phy-astr.gsu.edu/hbase/quantum/xtube.html. [Accessed: 18-Jan-2019]. [5] J. A. Seibert, “Flat-panel detectors: How much better are they?,” Pediatr. Radiol., vol. 36, no. SUPPL. 14, pp. 173–181, 2006. [6] E. N. Landis and D. T. Keane, “X-ray microtomography,” Mater. Charact., vol. 61, no. 12, pp. 1305–1316, 2010. [7] J. F. Barrett and N. Keat, “Artifacts in CT: Recognition and Avoidance,” RadioGraphics, vol. 24, no. 6, pp. 1679–1691, 2004. 4.8 References [1] E. N. Landis and D. T. Keane, “X-ray microtomography,” Mater. Charact., vol. 61, no. 12, pp. 1305–1316, 2010. [2] M. Naeimi, Z. Li, Z. Qian,Y. Zhou, J. Wu, R. H. Petrov, J. Sietsma and R. Dollevoet, “Reconstruction of the rolling contact fatigue cracks in rails using X-ray computed tomography” NDT E Int., vol. 92, no. April, pp. 199–212, 2017. [3] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part II : Growth,” vol. 47, pp. 373–381, 2013. [4] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [5] J. F. Barrett and N. Keat, “Artifacts in CT: Recognition and Avoidance,” RadioGraphics, vol. 24, no. 6, pp. 1679–1691, 2004. [6] NSW Transport RailCorp, “Rail Defects Handbook: TMC 226,” pp. 1–83, 2012. [7] X. Deng, Z. Qian, Z. Li, and R. Dollevoet, “Investigation of the formation of corrugation-induced rail Squats based on extensive field monitoring,” Int. J. Fatigue, vol. 112, no. February, pp. 94–105, 2018. [8] F. J. Franklin, I. Widiyarta, and A. Kapoor, “Computer simulation of wear and rolling contact fatigue,” Wear, vol. 250, no. 251, pp. 949–955, 2001. [9] D. Scott, D. I. Fletcher, and B. J. Cardwell, “Simulation Study of Thermally Initiated Rail Defects,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 228, no. 2, pp. 113–127, 2012. [10] N. Gao, R. S. Dwyer-Joyce, and D. G. G. Grieve, “Disc machine testing to assess the life of surface-damaged railway track,” Proc. Inst. Mech. Eng. Part F-Journal Rail Rapid Transit, vol. 215, no. 4, pp. 261–275, 2001. [11] Z. Li, X. Zhao, C. Esveld, R. Dollevoet, and M. Molodova, “An investigation into the causes of Squats-Correlation analysis and numerical modeling,” Wear, vol. 265, no. 9–10, pp. 1349–1355, 2008. [12] A. Kapoor, F. J. Franklin, S. K. Wong, and M. Ishida, “Surface roughness and plastic flow in rail wheel contact,” vol. 253, pp. 257–264, 2002. [13] H. M. Smith, “An examination of Squat defects in a 60E1 R260 rail removed from the Bussy Saint Georges test site in the Paris suburbs ( RER line ),” Rotherham, UK, 2011. [14] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [15] J. H. You, “Damage and fatigue crack growth of Eurofer steel first wall mock-up under cyclic heat flux loads. Part 2: Finite element analysis of damage evolution,” Fusion Eng. Des., vol. 89, no. 4, pp. 294–301, 2014. 5.11 References [1] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [2] S. Djaziri, Y. Li, G. A. Nematollahi, B. Grabowski, S. Goto, C. Kirchlechner, A. Kostka, S. Doyle, J. Neugebauer, D. Raabe, G. Dehm, “Deformation-Induced Martensite: A New Paradigm for Exceptional Steels,” Adv. Mater., vol. 28, no. 35, pp. 7753–7757, 2016. [3] S. Simon, “Thèse De la dynamique ferroviaire à l ’ accommodation microstructurale du rail,” 2014. [4] T. KUNIO, M. SHIMIZU, K. YAMADA, M. ENOMOTO, and A. YOSHITAKE, “the Role of Prior Austenite Grains in Fatigue Crack Initiation and Propagation in Low Carbon Martensite,” Fatigue Fract. Eng. Mater. Struct., vol. 2, no. 3, pp. 237–249, 1979. [5] T. E. Tallian, Failure Atlas for Hertz Contact Machine Elements. New York: ASME Press, 1992. [6] Y. Nakanishi, K. Sugimoto, and N. Morita, “Investigation for the Flashover Phenomenon in DC Machines,” IEEJ Trans. Ind. Appl., vol. 129, no. 11, pp. 1054–1059, 2009. [7] RAIB, “Uncontrolled evacuation of a London Underground train at Holland Park station 25 August 2013,” Derby, UK. [8] Y. C. Chiou, R. T. Lee, and S. M. Lin, “Formation mechanism of electrical damage on sliding lubricated contacts for steel pair under DC electric field,” Wear, vol. 266, no. 1–2, pp. 110–118, 2009. [9] N. Gao, R. S. Dwyer-Joyce, and D. G. Grieve, “Disk Machine Experiments to Assess the Life of Damaged Railway Track,” 2001. [10] J. H. You, “Damage and fatigue crack growth of Eurofer steel first wall mock-up under cyclic heat flux loads. Part 2: Finite element analysis of damage evolution,” Fusion Eng. Des., vol. 89, no. 4, pp. 294–301, 2014. [11] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. [12] M. Steenbergen, “Squat formation and rolling contact fatigue in curved rail track,” Eng. Fract. Mech., vol. 143, pp. 80–96, 2015. 6.6 References [1] M. Naeimi, Z. Li, and R. Dollevoet, “Nucleation of Squat cracks in rail, calculation of crack initiation angles in three dimensions,” J. Phys. Conf. Ser., vol. 628, p. 012043, 2015. [2] Y. Zhou, X. Zheng, J. Jiang, and D. Kuang, “Modeling of rail head checks by X-ray computed tomography scan technology,” Int. J. Fatigue, vol. 100, pp. 21–31, 2017. [3] S. Earl, K. E. Rankin, R. Lewis, L. Smith, and W. M. Rainforth, “Comparison of Squats and Studs from different traffic environments,” in Proceedings of the 11th International Conference on Contact Mechanics and Wear of Rail/wheel Systems, CM 2018, 2018. [4] Z. Popovic Radovic, V., “Analysis of cracking on running surface of rails,” Gradevinar, vol. 65, no. 3, pp. 251–259, 2013. [5] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [6] S. L. Grassie, “Studs and Squats: The evolving story,” Wear, vol. 366–367, pp. 194–199, 2016. [7] A. Ekberg, “D3.1- Enhanced track structure- Status, key influencing parameters and prioritised areas of improvement v.6,” 2018. [8] M. Steenbergen, “Rolling contact fatigue in relation to rail grinding,” Wear, vol. 356–357, pp. 110–121, 2016. [9] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part I : Origination,” vol. 47, pp. 361–372, 2013. [10] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. [11] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [12] A. Kapoor, F. J. Franklin, S. K. Wong, and M. Ishida, “Surface roughness and plastic flow in rail wheel contact,” vol. 253, pp. 257–264, 2002. 7.10. References [1] Z. Li, X. Zhao, C. Esveld, R. Dollevoet, and M. Molodova, “An investigation into the causes of Squats-Correlation analysis and numerical modeling,” Wear, vol. 265, no. 9–10, pp. 1349–1355, 2008. [2] Z. Li, “Squats on Railway Rails,” in Wheel-Rail Interface Handbook, R. Lewis and U. Olofsson, Eds. Woodhead Publishing Limited, 2009. 8.7 References [1] J. M. Cookson and P. Mutton, “The role of the environment in the rolling contact fatigue cracking of rails,” Wear, vol. 271, no. 1–2, pp. 113–119, 2011."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Eng.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.826851"]},{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["EP/L016273/1 for hte CDT AMS"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/28616/1/Shaun%20Earl%20Squats%20Thesis%20resubmission%20Jan%202021.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["This thesis contains the results from an investigation into Squats, a discrete rail steel defect. Micro-computed tomography (micro-CT) scanning was used to scan the entire structure of four out of five defects removed from railway track. The fifth was not scanned as it shelled in track. The difficulty turning these raw X-ray images into a segmented 3D model were overcome by developing a new technique. Isolating separate regions of the scans created areas where voxel value variation was at a minimum (i.e. the histogram became one narrow peak rather than multiple broad peaks). This allowed the automatic crack segregation module to work fairly well, and then enhanced using the region growing modules within the software. These scan results were then verified to be accurate using metallographic sample preparation, optical and electron microscopy. Micro CT scanning was performed on a custom 450KeV scanner, allowing the capture of the first entire Squat crack network morphology. Full defect imaging allowed the different defects to be compared to each other, highlighting differences and similarities. The defects came from metro, mixed and high-speed railways and one was found within an aluminothermic weld. The verification process and investigations of the scan volumes yielded further information about the defect’s origins. These origins were used to determine that, for the five defects investigated, there were four different causes. The two that shared a cause were from the same track section. Based on the causes, the defects were identified as a Stud, two Grinding Induced Squats (GIS), a Squat (caused by the legacy issue of MnS inclusions) and possibly a Squat or Stud in a slightly contaminated weld. None of the defects were considered to be a classic Squat, which is caused by Rolling Contact Fatigue (RCF), because there were other factors in their initiation. One of the defects contained a transverse defect, which is a crack that grows down through the railhead and can break the rail. This transverse defect was ~9mm deep into the rail when it was removed, meaning it would not have returned to the surface to shell. A high-resolution volume of the transverse defect region was created and its origin gives an important insight into the potential causes of rail-breaking defects. The origin of this transverse defect was a cluster of debris-filled voids that had formed due to the corrosion and cyclic loading (fretting) of a crack branch. These voids aligned with a deep grinding mark on the surface of the rail, which acted as a stress raiser. Because corrosion is a factor in this transverse defect case, the age of a rail and its environment are factors for defect development as well as traffic volume, given the correlation of corrosion with time. Results of this work highlight both the importance of a good surface finish and the diversity of causes found within the term “Squat”. Thus the identification of the Stud variant may be the beginning of a more comprehensive group of Squat type defects being established. This refining of the category could lead to fruitful big data analyses of the Squat type defect occurrences. The CT volumes of the defects created in this work can easily be stored for comparison in future investigations. The virtual nature of the volumes allows the sharing of defect information more readily than physical and sectioned defects, which deteriorate with time and require physical storage and transport."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Micro-CT Scanning in the Investigation of Squat Defects in Rail Steel"]}]}],"canonical_facts":{"dc:contributor.advisor":["Rainforth, W. Mark","Lewis, Roger","Smith, Lindsey"],"dc:contributor.sponsor":["ESPRC"],"dc:creator":["Earl, Shaun"],"dc:date":["2021-01"],"dc:date.issued":["2021-01"],"dc:description.abstract":["This thesis contains the results from an investigation into Squats, a discrete rail steel defect. Micro-computed tomography (micro-CT) scanning was used to scan the entire structure of four out of five defects removed from railway track. The fifth was not scanned as it shelled in track. The difficulty turning these raw X-ray images into a segmented 3D model were overcome by developing a new technique. Isolating separate regions of the scans created areas where voxel value variation was at a minimum (i.e. the histogram became one narrow peak rather than multiple broad peaks). This allowed the automatic crack segregation module to work fairly well, and then enhanced using the region growing modules within the software. These scan results were then verified to be accurate using metallographic sample preparation, optical and electron microscopy. Micro CT scanning was performed on a custom 450KeV scanner, allowing the capture of the first entire Squat crack network morphology. Full defect imaging allowed the different defects to be compared to each other, highlighting differences and similarities. The defects came from metro, mixed and high-speed railways and one was found within an aluminothermic weld. The verification process and investigations of the scan volumes yielded further information about the defect’s origins. These origins were used to determine that, for the five defects investigated, there were four different causes. The two that shared a cause were from the same track section. Based on the causes, the defects were identified as a Stud, two Grinding Induced Squats (GIS), a Squat (caused by the legacy issue of MnS inclusions) and possibly a Squat or Stud in a slightly contaminated weld. None of the defects were considered to be a classic Squat, which is caused by Rolling Contact Fatigue (RCF), because there were other factors in their initiation. One of the defects contained a transverse defect, which is a crack that grows down through the railhead and can break the rail. This transverse defect was ~9mm deep into the rail when it was removed, meaning it would not have returned to the surface to shell. A high-resolution volume of the transverse defect region was created and its origin gives an important insight into the potential causes of rail-breaking defects. The origin of this transverse defect was a cluster of debris-filled voids that had formed due to the corrosion and cyclic loading (fretting) of a crack branch. These voids aligned with a deep grinding mark on the surface of the rail, which acted as a stress raiser. Because corrosion is a factor in this transverse defect case, the age of a rail and its environment are factors for defect development as well as traffic volume, given the correlation of corrosion with time. Results of this work highlight both the importance of a good surface finish and the diversity of causes found within the term “Squat”. Thus the identification of the Stud variant may be the beginning of a more comprehensive group of Squat type defects being established. This refining of the category could lead to fruitful big data analyses of the Squat type defect occurrences. The CT volumes of the defects created in this work can easily be stored for comparison in future investigations. The virtual nature of the volumes allows the sharing of defect information more readily than physical and sectioned defects, which deteriorate with time and require physical storage and transport."],"dc:format":["text"],"dc:identifier":["uk.bl.ethos.826851"],"dc:identifier.grantnumber":["EP/L016273/1 for hte CDT AMS"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/28616/1/Shaun%20Earl%20Squats%20Thesis%20resubmission%20Jan%202021.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Materials Science and Engineering (Sheffield)","Mechanical Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/28616/"],"dc:relation.references":["1.4 References [1] Network Rail, “Rail Head Squats,” 2015. [Online]. Available: https://cdn.networkrail.co.uk/wp-content/uploads/2017/03/Challenge-Statement-Track-Plain-line-rail-head-squats.pdf. [Accessed: 13-Jun-2018]. [2] E. N. Landis and D. T. Keane, “X-ray microtomography,” Mater. Charact., vol. 61, no. 12, pp. 1305–1316, 2010. [3] C. Jessop, J. Ahlström, L. Hammar, S. Fæster, and H. K. Danielsen, “3D characterization of rolling contact fatigue crack networks,” Wear, vol. 366–367, pp. 392–400, 2016. [4] M. Naeimi et al., “Reconstruction of the rolling contact fatigue cracks in rails using X-ray computed tomography,” NDT E Int., vol. 92, no. April, pp. 199–212, 2017. [5] J. J. Kalker, Three-dimensional elastic bodies in rolling contact. Kluwer Academic Publishers, 1990. [6] B. L. Singh and C. B. E. Sr, “Rolling Contact Fatigue in Rails – an Overview,” 2008. [Online]. Available: http://www.iricen.gov.in/iricen/ipwe_seminar/2011/paper_2_lalloosingh.pdf. [Accessed: 17-Jul-2020]. [7] W. Daniel, S. Pal, and M. . Farjoo, “Rail squats: progress in understanding the Australian experience,” J. Rail Rapid Transit, vol. 227, no. 5, pp. 481–492, 2013. [8] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. 2.9 References [1] Network Rail, “Rail Head Squats,” 2015. [Online]. Available: https://cdn.networkrail.co.uk/wp-content/uploads/2017/03/Challenge-Statement-Track-Plain-line-rail-head-Squats.pdf. [Accessed: 13-Jun-2018]. [2] K. L. Johnson, Contact Mechanics. Cambridge University Press, 1985. [3] H. Wu and N. Wilson, “Flange climb derailments: causes and prevention,” Int. Railw. J., vol. 52, no. 3, p. 47, 2012. [4] D. I. Fletcher and J. Beynon, “Development of a Machine for Closely Controlled Rolling Contact Fatigue and Wear Testing.,” J. Test. Eval., vol. 28, no. 4, p. 267, 2000. [5] R. S. Dwyer-Joyce, C. Yao, and R. Lewis, “A Comparison of Three Methods for the Measurement of Wheel Rail Contact,” STLE/ASME 2008 Int. Jt. Tribol. Conf., no. November 2015, pp. 541–543, 2008. [6] J. J. Kalker, Three-dimensional elastic bodies in rolling contact. Kluwer Academic Publishers, 1990. [7] J. J. Kalker, “A fast algorithm for the simplified theory of rolling contact,” Veh. Syst. Dyn., vol. 11, no. 1, 1982. [8] J. Srivastava, P. Sarkar, and V. Ranjan, “A numerical study on effects of friction-induced thermal load for rail under varied wheel slip conditions,” Simul. Trans. ofthe Soc. Model. Simul. Int., pp. 1–12, July 2018. [9] T. Telliskivi and U. Olofsson, “Contact mechanics analysis of measured wheel-rail profiles using the finite element method,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 215, no. 2, pp. 65–72, 2001. [10] A. Kapoor, F. J. Franklin, S. K. Wong, and M. Ishida, “Surface roughness and plastic flow in rail wheel contact,” vol. 253, pp. 257–264, 2002. [11] F. J. Franklin, I. Widiyarta, and A. Kapoor, “Computer simulation of wear and rolling contact fatigue,” Wear, vol. 250-251, pp. 949–955, 2001. [12] O. Arias-Cuevas, Z. Li, R. Lewis, and E. A. Gallardo-Hernández, “Rolling-sliding laboratory tests of friction modifiers in dry and wet wheel-rail contacts,” Wear, vol. 268, no. 3–4, pp. 543–551, 2010. [13] J. H. Al-Bedhany and H. Long, “Microscopic investigation of subsurface initiated damage of wind turbine gearbox bearings,” J. Phys. Conf. Ser., vol. 1106, no. 1, p.12029, 2018. [14] E. Magel and J. Kalousek, “Martensite and Contact Fatigue Initiated Wheel Defects,” in 12th International Wheelset Congress, 1998, pp. 100–111. [15] J. A. Williams, “The influence of repeated loading , residual stresses and shakedown on the behaviour of tribological contacts,” vol. 38, pp. 786–797, 2005. [16] E. Magel, “Rolling Contact Fatigue: A Comprehensive Review,” ECS Trans., vol. 28, no. 32, pp. 35–44, 2010. [17] S. R. Lewis, R. Lewis, and D. I. Fletcher, “Assessment of laser cladding as an option for repairing/enhancing rails,” Wear, vol. 330–331, no. July, pp. 581–591, 2015. [18] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [19] F. . Carter, “On the Action of a Locomotive Driving Wheel,” Proc. R. Soc., vol. A112, pp. 151–157, 1926. [20] J. J. Kalker, “Wheel — rail rolling contact theory,” vol. 144, pp. 243–261, 1991. [21] L. Smith, “Rolling Contact Fatigue in Wheel-Rail Contact,” University of Newcastle Upon Tyne, 2007. [22] R. Lewis and U. Olofsson, “Chapter 5: Tribology of the Wheel–Rail Contact,” in Handbook of Railway Vehicle Dynamics, S. Iwnicki, M. Spiryagin, C. Cole, and T. McSweeney, Eds. Taylor & Francis Group, LLC, 2006, p. 131. [23] R. Stock, L. Stanlake, C. Hardwick, M. Yu, D. Eadie, and R. Lewis, “Material concepts for top of rail friction management – Classification, characterisation and application,” Wear, vol. 366–367, pp. 225–232, 2016. [24] R. Stock, D. T. Eadie, D. Elvidge, and K. Oldknow, “Influencing rolling contact fatigue through top of rail friction modifier application - A full scale wheel-rail test rig Study,” Wear, vol. 271, no. 1–2, pp. 134–142, 2011. [25] J. Williams, Rolling contacts and rolling-element bearings. Cambridge University Press. [26] D. I. Fletcher and J. Beynon, “The effect of intermittent lubrication on the fatigue life of pearlitic rail steel in rolling- sliding contact,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 214, pp. 145–158, 2000. [27] M. Kaneta, K. Matsudo, K. Murakami, and H. Nishikawa, “1998 ASME Kaneta A Possible Mechanism.pdf,” ASME, vol. 120, pp. 304–309, 1998. [28] S. Bogda, P. Lewicki, and M. Szymaniak, “Experimental and theoretical investigation of the phenomenon of filling the RCF crack with liquid,” vol. 258, pp. 1280–1287, 2005. [29] N. Gao, R. S. Dwyer-Joyce, and D. G. G. Grieve, “Disc machine testing to assess the life of surface-damaged railway track,” Proc. Inst. Mech. Eng. Part F-Journal Rail Rapid Transit, vol. 215, no. 4, pp. 261–275, 2001. [30] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [31] C. Hardwick, R. Lewis, and R. Stock, “The effects of friction management materials on rail with pre existing rcf surface damage,” Wear, vol. 384–385, no. November 2016, pp. 50–60, 2017. [32] M. Sol-Sánchez, F. Moreno-Navarro, and M. C. Rubio-Gámez, “Analysis of ballast tamping and stone-blowing processes on railway track behaviour: the influence of using USPs,” Géotechnique, vol. 66, no. 6, pp. 481–489, 2016. [33] E. T. (Ernest T. Selig and J. M. Waters, Track geotechnology and substructure management. Thomas Telford, 1994. [34] J. Miss, “Running Surface Features and Defect Catalogue,” pp. 1-71, 2010. [35] NSW Transport RailCorp, “Rail Defects Handbook: TMC 226,” pp. 1–83, 2012. [36] P. Mutton, J. Cookson, C. Qiu, and D. Welsby, “Microstructural characterisation of rolling contact fatigue damage in flashbutt welds,” Wear, vol. 366–367, pp. 368–377, 2016. [37] E. Magel, M. Roney, J. Kalousek, and P. Sroba, “The blending of theory and practice in modern rail grinding,” Fatigue Fract. Eng. Mater. Struct., vol. 26, no. 10, pp. 921–929, 2003. [38] Bhadeshia, Harshad K. D. H., et al. Steels: Microstructure and Properties, Elsevier Science & Technology, 2006. [39] D. Aliya and A. Analytical, “Physical Metallurgy Concepts in Interpretation of Microstructures,” Metallogr. Microstruct., vol. 9, pp. 44–70, 2018. [40] University of Cambridge, “Interpretation of cooling curves.” [Online]. Available: https://www.doitpoms.ac.uk/tlplib/phase-diagrams/cooling.php. [Accessed: 29-Apr-2019]. [41] F. P. L. Kavishe and T. J. Baker, “Effect of prior austenite grain size and pearlite interlamellar spacing on strength and fracture toughness of a eutectoid rail steel,” Mater. Sci. Technol., vol. 2, no. 8, pp. 816–822, 2014. [42] H. W. Zhang, S. Ohsaki, S. Mitao, M. Ohnuma, and K. Hono, “Microstructural investigation of white etching layer on pearlite steel rail,” Mater. Sci. Eng. A, vol. 421, no. 1–2, pp. 191–199, 2006. [43] G. E. Totten and G. E. Totten, “Failures Related to Heat Treating Operations,” Fail. Anal. Prev., vol. 11, pp. 192–223, 2018. [44] International Union of Railways, “INNOTRACK concluding technical report,” Paris, France, 2010. [45] ARTC, “Rail Defects Handbook Some Rail Defects , their Characteristics , Causes and Control RC 2400,” no. March, 2006. [46] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. [47] V. Dikshit, P. Clayton, and D. Christensen, “Investigation of rolling contact fatigue in a head-hardened rail,” Wear, vol. 144, no. 1–2, pp. 89–102, 1991. [48] TataSteel, “Review of anti Squat research,” 2013. [49] R. Stock and R. Pippan, “Rail grade dependent damage behaviour – Characteristics and damage formation hypothesis,” Wear, vol. 314, no. 1–2, pp. 44–50, 2014. [50] W. Solano-Alvarez and H. K. D. H. Bhadeshia, “White-etching matter in bearing steel. Part I: Controlled cracking of 52100 steel,” Metall. Mater. Trans. A Phys. Metall. Mater. Sci., vol. 45, no. 11, pp. 4907–4915, 2014. [51] P. Clayton and M. B. P. Allery, “Metallurgical Aspects of Surface Damage Problems in Rails,” Can. Metall. Q., vol. 21, no. 1, pp. 31–46, 1982. [52] UIC, “Recommendations for the use of rail steel grades,” pp. 4, 2015. [53] E. Magel, P. Sroba, K. Sawley, and J. Kalousek, “Control of Rolling Contact Fatigue of Rails,”, pp. 8, 2005. [54] J. E. Garnham and C. L. Davis, “Very early stage rolling contact fatigue crack growth in pearlitic rail steels,” Wear, vol. 271, no. 1–2, pp. 100–112, 2011. [55] M. Burstow, “Experience of premium grade rail steels to resist rolling contact fatigue (RCF) on GB network,” Ironmak. Steelmak., vol. 40, no. 2, pp. 103–107, 2013. [56] A. D. Hearle and K. L. Johnson, “Mode II stress intensity factors for a crack parallel to the surface of an elastic half-space subjected to a moving point load,” J. Mech. Phys. Solids, vol. 33, no. 1, pp. 61–81, Jan. 1985. [57] A. Kapoor, D. I. Fletcher, and F. J. Franklin, “The role of wear in enhancing rail life,” Tribol. Ser., no. 41, pp. 331–340, 2002. [58] J. E. Garnham and J. Beynon, “The early detection of rolling-sliding contact fatigue cracks,” Wear, vol. 144, no. 1–2, pp. 103–116, 1991. [59] D. I. Fletcher, P. Hyde, and A. Kapoor, “Investigating fluid penetration of rolling contact fatigue cracks in rails using a newly developed full-scale test facility,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 221, pp. 35–44, 2007. [60] A. J. Perez-Unzueta and J. H. Beynon, “Microstructure and wear resistance of pearlitic rail steels.pdf,” Wear, vol. 162–164, pp. 173–82, 1993. [61] P. Clayton, “Tribological aspects of wheel-rail contact: a review of recent experimental research,” Wear, vol. 191, pp. 170–183, 1996. [62] J. F. Archard and W. Hirst, “The wear of metals under unlubricated conditions,” Proc. R. Soc. London., vol. 236, no. Ser. A. Math. Phys. Sci., pp. 397–410, 1956. [63] D. F. Cannon, K. O. Edel, S. L. Grassie, and K. Sawley, “Rail defects: An overview,” Fatigue Fract. Eng. Mater. Struct., vol. 26, no. 10, pp. 865–886, 2003. [64] S. B. Newcomb and W. M. Stobbs, “A transmission electron microscope Study of the white etching layer on a rail head,” Mater. Sci. Eng. A, vol. 66, pp. 195–204, 1984. [65] J. Wu, R. H. Petrov, M. Naeimi, Z. Li, R. Dollevoet, and J. Sietsma, “Laboratory simulation of martensite formation of white etching layer in rail steel,” Int. J. Fatigue, vol. 91, pp. 11–20, 2016. [66] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part I : Origination,” vol. 47, pp. 361–372, 2013. [67] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [68] S. Simon. De la dynamique ferroviaire `a l’accommodation microstructurale du rail : Contribution des TTS `a la r´eponse tribologique des aciers : Cas du d´efaut de squat. Mechanics of the solides. INSA de Lyon, 2014. French. [69] A. Al-juboori et al., “Squat formation and the occurrence of two distinct classes of white etching layer on the surface of rail steel,” vol. 104, pp. 52–60, 2017. [70] W. Lojkowski, M. Djahanbakhsh, G. Bürkle, S. Gierlotka, W. Zielinski, and H. J. Fecht, “Nanostructure formation on the surface of railway tracks,” Mater. Sci. Eng. A, vol. 303, no. 1–2, pp. 197–208, 2001. [71] S. Simon, A. Saulot, C. Dayot, X. Quost, and Y. Berthier, “Tribological characterization of rail Squat defects,” Wear, vol. 297, no. 1–2, pp. 926–942, 2013. [72] R. I. Carroll, “Surface Metallurgy and Rolling Contact Fatigue of Rail,” University of Sheffield, 2005. [73] F. Alwahdi, “Wear and Rolling Contact Fatigue of Ductile Materials,” University of Sheffield, 2004. [74] A. Ekberg, “D3.1- Enhanced track structure- Status, key influencing parameters and prioritised areas of improvement v.6,” pp. 11-12, 2018. [75] S. Li, J. Wu, R. H. Petrov, Z. Li, R. Dollevoet, and J. Sietsma, “‘Brown etching layer’: A possible new insight into the crack initiation of rolling contact fatigue in rail steels?,” Eng. Fail. Anal., vol. 66, pp. 8–18, 2016. [76] M. Steenbergen, “Squat formation and rolling contact fatigue in curved rail track,” Eng. Fract. Mech., vol. 143, pp. 80–96, 2015. [77] S. L. Grassie, “Rail corrugation: characteristics, causes, and treatments,” Proc. IMechE Vol. 223 Part F J. Rail Rapid Transit, pp. 581–596, 2009. [78] K. Kondo, K. Yoroizaka, and Y. Sato, “Cause, increase, diagnosis, countermeasures and elimination of Shinkansen shelling,” Wear, vol. 191, no. 1–2, pp. 99–203, 1996. [79] F. Fau, H. Smith, S. Fretwell-Smith, L. Deng, “Effect of grinding quality, lubri- cation quality and rail hardness on flaking defect initiation on high rails” Proceedings of the 10th International Conference on Contact Mechanics and Wear of Rail/Wheel Systems (CM2015), Colorado, USA, 30 August–3 September. [80] M. Steenbergen, “Rolling contact fatigue in relation to rail grinding,” Wear, vol. 356–357, pp. 110–121, 2016. [81] A. C. Athukorala, “Investigation of Wear and Ratcheting Response of Head-Hardened Australian Rail Steel under Conditions of Rolling Contact Fatigue,” Queensland University of Technology SCIENCE, 2016. [82] S. L. Grassie, “Squats and Squat-type defects in rails: the understanding to date,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 235–242, 2012. [83] S. L. Grassie, “Studs and Squats: The evolving story,” Wear, vol. 366–367, pp. 194–199, 2016. [84] M. Ishida, “Rolling contact fatigue (RCF) defects of rails in Japanese railways and its mitigation strategies,” Electron. J. Struct. Eng., vol. 13, no. 1, pp. 67–74, 2013. [85] S. L. Grassie, “Rolling contact fatigue on the British railway system : treatment,” vol. 258, no. June 2003, pp. 1310–1318, 2005. [86] Railtrack plc, Rolling contact fatigue in rails: a guide to current understanding and practice. Heron Press, Birmingham, UK, 2001. [87] M. Kerr, A. Wilson, and S. Marich, “The epidemiology of Squats and related rail defects,” CORE 2008 Conf. Railw. Eng. rail- the-core Integr. Transp., no. September, pp. 83–96, 2008. [88] S. Kaewunruen, M. Ishida. In Situ Monitoring of Rail Squats in Three Dimensions Using Ultrasonic Technique. Exp Tech 40, 1179–1185 (2016). [89] X. Zhao, Dynamic Wheel/Rail Rolling Contact at Singular Defects with Application on Squats. Southwest Jiaotong University, 2012. [90] M. Ishida, M. Akama, K. Kashiwaya, and A. Kapoor, “The current status of theory and practice on rail integrity in Japanese railways-rolling contact fatigue and corrugations,” Fatigue Fract. Eng. Mater. Struct., vol. 26, no. 10, pp. 909–919, 2003. [91] S. Kaewunruen, “Identification and prioritization of rail Squat defects in the field using rail magnetisation technology,” Struct. Heal. Monit. Insp. Adv. Mater. Aerospace, Civ. Infrastruct. 2015, vol. 9437, no. April 2015, p. 94371H, 2015. [92] S. Kaewunruen and M. Ishida, “Rail Squats: understand its causes, severity , and non-destructive evaluation techniques,” Proceedings of the 20th National Convention on Civil Engineering Vol. 1 Iss. 1, 2015. [93] Z. Li, X. Zhao, C. Esveld, R. Dollevoet, and M. Molodova, “An investigation into the causes of Squats-Correlation analysis and numerical modeling,” Wear, vol. 265, no. 9–10, pp. 1349–1355, 2008. [94] M. Kerr and W. Daniel, “Final Report on the Rail Squat Project R3-105,” CRC for Rail Innovation, Brisbane, 2011. [95] L. Deng, “Understanding of rail Squats from the point of view of metallurgy, Tata Steel internal presentation.” . [96] Z. Li, “Squats on Railway Rails,” in Wheel-Rail Interface Handbook, R. Lewis and U. Olofsson, Eds. Woodhead Publishing Limited, 2009. [97] E. Magel, P. Mutton, A. Ekberg, and A. Kapoor, “Rolling contact fatigue, wear and broken rail derailments,” Wear, vol. 366–367, pp. 249–257, 2016. [98] C. J. Rasmussen, X. Zhang, H. K. Danielsen, and S. Fæster, “Grinding induced martensite on the surface of rails,” Proc. 35th Risø Int. Symp. Mater. Sci. New Front. Nanometals, vol. 35, pp. 439–446, 2014. [99] M. Farjoo, W. Daniel, P. Bellette, and P. A. Meehan, “Field statistical and finite element analysis of rail Squats,” Eng. Fract. Mech., vol. 109, pp. 117–129, 2013. [100] Z. Li, R. Dollevoet, M. Molodova, and X. Zhao, “Squat growth — Some observations and the validation of numerical predictions,” Wear, vol. 271, no. 1–2, pp. 148–157, 2011. [101] M. Naeimi et al., “Reconstruction of the rolling contact fatigue cracks in rails using X-ray computed tomography,” NDT E Int., vol. 92, no. April, pp. 199–212, 2017. [102] C. Jessop, J. Ahlström, L. Hammar, S. Fæster, and H. K. Danielsen, “3D characterization of rolling contact fatigue crack networks,” Wear, vol. 366–367, pp. 392–400, 2016. [103] N. Gao, R. S. Dwyer-Joyce, and D. G. G. Grieve, “Disc machine testing to assess the life of surface-damaged railway track,” Proc. Inst. Mech. Eng. Part F-Journal Rail Rapid Transit, vol. 215, no. 4, pp. 261–275, 2001. [104] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part II : Growth,” vol. 47, pp. 373–381, 2013. [105] D. I. Fletcher and S. H. Sanusi, “the Potential for Supressing Rail Defect Growth Through Tailoring Rail Thermo-Mechanical Properties,” in 10th International Conference on Contact Mechanics and Wear of Rail/ Wheel System, 2015. [106] D. Scott, D. I. Fletcher, and B. J. Cardwell, “Simulation Study of Thermally Initiated Rail Defects,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 228, no. 2, pp. 113–127, 2012. [107] M. Kerr and A. Wilson, “Rail Squat Defects,” Perm. W. Inst. Inc, pp. 13–25, 2000. [108] Sperry Rail Service, “Rail Defect Manual,” p. 43, 1968. [109] Federal Railroad Administration, “Track Inspector Rail Defect Reference Manual,” 2015. [110] H. M. Smith, “An examination of Squat defects in a 60E1 R260 rail removed from the Bussy Saint Georges test site in the Paris suburbs ( RER line ),” Rotherham, UK, 2011. [111] M. Itabashi and K. Kawata, “Carbon content effect on high-strain-rate tensile properties for carbon steels,” Int. J. Impact Eng., vol. 24, no. 2, pp. 117–131, 2000. [112] Z. Popovic Radovic, V., “Analysis of cracking on running surface of rails,” Gradevinar, vol. 65, no. 3, pp. 251–259, 2013. [113] T. Szugs et al., “Combination of Ultrasonic and Eddy Current Testing with Imaging for Characterization of Rolling Contact Fatigue,” 19th World Conference on Non-Destructive Testing (WCNDT 2016), 13-17 June 2016 in Munich, Germany (WCNDT), 2016. [114] D. Peng and R. Jones, “Lock-in thermographic inspection of Squats on rail steel head,” Infrared Phys. Technol., vol. 57, pp. 89–95, 2013. [115] M. Molodova, Z. Li, A. Nunez, and R. Dollevoet, “Automatic Detection of Squats in Railway Infrastructure,” IEEE Traansactions Intell. Transp. Syst., vol. 15, no. 1, pp. 1980–1990, 2014. [116] Network Rail, “Re-Profiling Rail to Remove Defects & Extend Rail Life.” [Online]. Available: https://www.networkrail.co.uk/wp-content/uploads/2019/06/Challenge-statement-track-re-profiling-rail-to-remove-defects-and-extend-rail-life.pdf. [Accessed: 19-Aug-2019]. [117] Taubert, M. “High-speed grinding.” International Railway Journal, 45(12), p.40-41, 2005. [118] Network Rail, “Innovative, new grinding trains will help passenger and freight trains run smoothly and safely for years to come.” [Online]. Available: https://www.networkrailmediacentre.co.uk/news/innovative-new-grinding-trains-will-help-passenger-and-freight-trains-run-smoothly-and-safely-for-years-to-come. [Accessed: 09-Aug-2019]. [119] A. Faley, “Repair of a ‘Squat’ defect by thermit welding,” no. 919, pp. 95–97, 1979. 3.6 References [1] A. H. Compton and D. Ph, “THE SCATTERING OF X-RAYS TIIE present paper will be confined to a discussion of some of the points which present to us a revolutionary change in our ideas regarding the process of scattering of electromagnetic waves . No attempt will be made to describe t,” vol. 198, no. 1183, 1923. [2] Iowa State University NDT Education Resource Centre, “Sources of Attenuation,” 2014. [Online]. Available: https://www.nde-ed.org/EducationResources/CommunityCollege/Radiography/Physics/attenuation.htm. [Accessed: 07-Jul-2019]. [3] H. Chen, M. M. Rogalski, and J. N. Anker, “Advances in functional X-ray imaging techniques and contrast agents,” Phys. Chem. Chem. Phys., vol. 14, no. 39, pp. 13469–13486, 2012. [4] R. Nave, “X-ray production.” [Online]. Available: http://hyperphysics.phy-astr.gsu.edu/hbase/quantum/xtube.html. [Accessed: 18-Jan-2019]. [5] J. A. Seibert, “Flat-panel detectors: How much better are they?,” Pediatr. Radiol., vol. 36, no. SUPPL. 14, pp. 173–181, 2006. [6] E. N. Landis and D. T. Keane, “X-ray microtomography,” Mater. Charact., vol. 61, no. 12, pp. 1305–1316, 2010. [7] J. F. Barrett and N. Keat, “Artifacts in CT: Recognition and Avoidance,” RadioGraphics, vol. 24, no. 6, pp. 1679–1691, 2004. 4.8 References [1] E. N. Landis and D. T. Keane, “X-ray microtomography,” Mater. Charact., vol. 61, no. 12, pp. 1305–1316, 2010. [2] M. Naeimi, Z. Li, Z. Qian,Y. Zhou, J. Wu, R. H. Petrov, J. Sietsma and R. Dollevoet, “Reconstruction of the rolling contact fatigue cracks in rails using X-ray computed tomography” NDT E Int., vol. 92, no. April, pp. 199–212, 2017. [3] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part II : Growth,” vol. 47, pp. 373–381, 2013. [4] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [5] J. F. Barrett and N. Keat, “Artifacts in CT: Recognition and Avoidance,” RadioGraphics, vol. 24, no. 6, pp. 1679–1691, 2004. [6] NSW Transport RailCorp, “Rail Defects Handbook: TMC 226,” pp. 1–83, 2012. [7] X. Deng, Z. Qian, Z. Li, and R. Dollevoet, “Investigation of the formation of corrugation-induced rail Squats based on extensive field monitoring,” Int. J. Fatigue, vol. 112, no. February, pp. 94–105, 2018. [8] F. J. Franklin, I. Widiyarta, and A. Kapoor, “Computer simulation of wear and rolling contact fatigue,” Wear, vol. 250, no. 251, pp. 949–955, 2001. [9] D. Scott, D. I. Fletcher, and B. J. Cardwell, “Simulation Study of Thermally Initiated Rail Defects,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 228, no. 2, pp. 113–127, 2012. [10] N. Gao, R. S. Dwyer-Joyce, and D. G. G. Grieve, “Disc machine testing to assess the life of surface-damaged railway track,” Proc. Inst. Mech. Eng. Part F-Journal Rail Rapid Transit, vol. 215, no. 4, pp. 261–275, 2001. [11] Z. Li, X. Zhao, C. Esveld, R. Dollevoet, and M. Molodova, “An investigation into the causes of Squats-Correlation analysis and numerical modeling,” Wear, vol. 265, no. 9–10, pp. 1349–1355, 2008. [12] A. Kapoor, F. J. Franklin, S. K. Wong, and M. Ishida, “Surface roughness and plastic flow in rail wheel contact,” vol. 253, pp. 257–264, 2002. [13] H. M. Smith, “An examination of Squat defects in a 60E1 R260 rail removed from the Bussy Saint Georges test site in the Paris suburbs ( RER line ),” Rotherham, UK, 2011. [14] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [15] J. H. You, “Damage and fatigue crack growth of Eurofer steel first wall mock-up under cyclic heat flux loads. Part 2: Finite element analysis of damage evolution,” Fusion Eng. Des., vol. 89, no. 4, pp. 294–301, 2014. 5.11 References [1] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [2] S. Djaziri, Y. Li, G. A. Nematollahi, B. Grabowski, S. Goto, C. Kirchlechner, A. Kostka, S. Doyle, J. Neugebauer, D. Raabe, G. Dehm, “Deformation-Induced Martensite: A New Paradigm for Exceptional Steels,” Adv. Mater., vol. 28, no. 35, pp. 7753–7757, 2016. [3] S. Simon, “Thèse De la dynamique ferroviaire à l ’ accommodation microstructurale du rail,” 2014. [4] T. KUNIO, M. SHIMIZU, K. YAMADA, M. ENOMOTO, and A. YOSHITAKE, “the Role of Prior Austenite Grains in Fatigue Crack Initiation and Propagation in Low Carbon Martensite,” Fatigue Fract. Eng. Mater. Struct., vol. 2, no. 3, pp. 237–249, 1979. [5] T. E. Tallian, Failure Atlas for Hertz Contact Machine Elements. New York: ASME Press, 1992. [6] Y. Nakanishi, K. Sugimoto, and N. Morita, “Investigation for the Flashover Phenomenon in DC Machines,” IEEJ Trans. Ind. Appl., vol. 129, no. 11, pp. 1054–1059, 2009. [7] RAIB, “Uncontrolled evacuation of a London Underground train at Holland Park station 25 August 2013,” Derby, UK. [8] Y. C. Chiou, R. T. Lee, and S. M. Lin, “Formation mechanism of electrical damage on sliding lubricated contacts for steel pair under DC electric field,” Wear, vol. 266, no. 1–2, pp. 110–118, 2009. [9] N. Gao, R. S. Dwyer-Joyce, and D. G. Grieve, “Disk Machine Experiments to Assess the Life of Damaged Railway Track,” 2001. [10] J. H. You, “Damage and fatigue crack growth of Eurofer steel first wall mock-up under cyclic heat flux loads. Part 2: Finite element analysis of damage evolution,” Fusion Eng. Des., vol. 89, no. 4, pp. 294–301, 2014. [11] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. [12] M. Steenbergen, “Squat formation and rolling contact fatigue in curved rail track,” Eng. Fract. Mech., vol. 143, pp. 80–96, 2015. 6.6 References [1] M. Naeimi, Z. Li, and R. Dollevoet, “Nucleation of Squat cracks in rail, calculation of crack initiation angles in three dimensions,” J. Phys. Conf. Ser., vol. 628, p. 012043, 2015. [2] Y. Zhou, X. Zheng, J. Jiang, and D. Kuang, “Modeling of rail head checks by X-ray computed tomography scan technology,” Int. J. Fatigue, vol. 100, pp. 21–31, 2017. [3] S. Earl, K. E. Rankin, R. Lewis, L. Smith, and W. M. Rainforth, “Comparison of Squats and Studs from different traffic environments,” in Proceedings of the 11th International Conference on Contact Mechanics and Wear of Rail/wheel Systems, CM 2018, 2018. [4] Z. Popovic Radovic, V., “Analysis of cracking on running surface of rails,” Gradevinar, vol. 65, no. 3, pp. 251–259, 2013. [5] S. L. Grassie, D. I. Fletcher, E. A. Gallardo Hernandez, and P. Summers, “Studs: a Squat-type defect in rails,” Proc. Inst. Mech. Eng. Part F J. Rail Rapid Transit, vol. 226, no. 3, pp. 243–256, 2011. [6] S. L. Grassie, “Studs and Squats: The evolving story,” Wear, vol. 366–367, pp. 194–199, 2016. [7] A. Ekberg, “D3.1- Enhanced track structure- Status, key influencing parameters and prioritised areas of improvement v.6,” 2018. [8] M. Steenbergen, “Rolling contact fatigue in relation to rail grinding,” Wear, vol. 356–357, pp. 110–121, 2016. [9] M. Steenbergen and R. Dollevoet, “On the mechanism of Squat formation on train rails – Part I : Origination,” vol. 47, pp. 361–372, 2013. [10] M. Steenbergen, “Rolling contact fatigue: Spalling versus transverse fracture of rails,” Wear, vol. 380–381, pp. 96–105, 2017. [11] C. Bernsteiner, G. Muller, A. Meierhofer, K. Six, D. Kunstner, and P. Dietmaier, “Development of white etching layers on rails: simulations and experiments,” Wear, vol. 366–367, pp. 116–122, 2016. [12] A. Kapoor, F. J. Franklin, S. K. Wong, and M. Ishida, “Surface roughness and plastic flow in rail wheel contact,” vol. 253, pp. 257–264, 2002. 7.10. References [1] Z. Li, X. Zhao, C. Esveld, R. Dollevoet, and M. Molodova, “An investigation into the causes of Squats-Correlation analysis and numerical modeling,” Wear, vol. 265, no. 9–10, pp. 1349–1355, 2008. [2] Z. Li, “Squats on Railway Rails,” in Wheel-Rail Interface Handbook, R. Lewis and U. Olofsson, Eds. Woodhead Publishing Limited, 2009. 8.7 References [1] J. M. Cookson and P. Mutton, “The role of the environment in the rolling contact fatigue cracking of rails,” Wear, vol. 271, no. 1–2, pp. 113–119, 2011."],"dcterms:accessrights":["public"],"dc:title":["Micro-CT Scanning in the Investigation of Squat Defects in Rail Steel"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Eng.D"]},"updated_at":"2026-11-18T22:41:49Z"}