{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:31413"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:31413","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Optimising the Laser Powder Bed Fusion Process for the Manufacture of a Nickel Superalloy","abstract":"Laser Powder bed Fusion as a form of additive manufacturing is a potentially desirable method of manufacture for aircraft parts that use nickel superalloys. One of the barriers to greater adoption is the uncertainty in mechanical properties build quality and microstructure that can arise from the LPBF process. This project explores how this uncertainty can be reduced or eliminated. Different methods achieve this reduction in uncertainty. A method for characterising both the laser and scanner system is outlined and tested. The different melting modes that can occur between the laser and the material are investigated. A closed-loop control system that included a machine learning algorithm was successfully implemented. This control had a statistically significant effect on reducing the variation in thermal emissivities. Constraints found from experimental observations and fundamental physics were imposed to reduce the creation of defects. The mechanical performance of Haynes 282 was benchmarked against other manufacturing methods and other alloys to find that test samples built using LPBF performed as well as wrought or cast samples in elevated stress rupture testing. In order to improve mechanical properties such as high temperature stress rupture resistance, the susceptibility of Haynes 282 to different cracking mechanisms was investigated. This susceptibility was tested through models and analysis of the microstructure and cracks themselves. The susceptibility was tested at different beam velocities, and it was found that the thermal front velocity was found to be critical in influencing the likelihood of crack formation. When the results of these experiments are combined, it suggests parameter ranges that suit both the alloy and the machine, whilst the closed-loop control can stay within these ranges even when the geometry or process conditions vary. This project was funded by GKN Aerospace in conjunction with the Engineering and Physical Sciences Research Council (EPSRC).","abstract_html":"Laser Powder bed Fusion as a form of additive manufacturing is a potentially desirable method of manufacture for aircraft parts that use nickel superalloys. One of the barriers to greater adoption is the uncertainty in mechanical properties build quality and microstructure that can arise from the LPBF process. This project explores how this uncertainty can be reduced or eliminated. Different methods achieve this reduction in uncertainty. A method for characterising both the laser and scanner system is outlined and tested. The different melting modes that can occur between the laser and the material are investigated. A closed-loop control system that included a machine learning algorithm was successfully implemented. This control had a statistically significant effect on reducing the variation in thermal emissivities. Constraints found from experimental observations and fundamental physics were imposed to reduce the creation of defects. The mechanical performance of Haynes 282 was benchmarked against other manufacturing methods and other alloys to find that test samples built using LPBF performed as well as wrought or cast samples in elevated stress rupture testing. In order to improve mechanical properties such as high temperature stress rupture resistance, the susceptibility of Haynes 282 to different cracking mechanisms was investigated. This susceptibility was tested through models and analysis of the microstructure and cracks themselves. The susceptibility was tested at different beam velocities, and it was found that the thermal front velocity was found to be critical in influencing the likelihood of crack formation. When the results of these experiments are combined, it suggests parameter ranges that suit both the alloy and the machine, whilst the closed-loop control can stay within these ranges even when the geometry or process conditions vary. This project was funded by GKN Aerospace in conjunction with the Engineering and Physical Sciences Research Council (EPSRC).","abstract_has_math":false,"creators":["Lyle, Alistair"],"institution":"University of Sheffield","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Iain, Todd","Katerina, Christofidou"],"committee_chairs":[],"committee_members":[],"year":2021,"date_issued":"2021-12","date_published":"2021-12","updated_at":"2026-11-18T23:19:31Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.878115"],"render_values":[{"text":"uk.bl.ethos.878115","href":null,"code":true}]}],"person_identifier_entries":[{"key":"person:identifier.orcid","label":"ORCID","values":["0000000316373525"],"render_values":[{"text":"0000-0003-1637-3525","href":"https://orcid.org/0000-0003-1637-3525","code":true}]}]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/31413/1/Lyle%20-%202021-%20Optimising%20the%20Laser%20Powder%20Bed%20Fusion%20Process%20for%20the%20Manufacture%20of%20a%20Nickel%20Superalloy.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A31413","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Iain, Todd","Katerina, Christofidou"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["EPSRC"]},{"key":"dc:creator","label":"Author","values":["Lyle, Alistair"]},{"key":"person:identifier.orcid","label":"ORCID","values":["0000000316373525"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2021-12"]},{"key":"dc:date.issued","label":"Date","values":["2021-12"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Materials Science and Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/31413/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["[1] C. T. Sims, “A history of superalloy metallurgy for superalloy metallurgists,” Superalloys, vol. 1984, pp. 399–419, 1984. [2] Y. J. Liu et al., “Microstructure, defects and mechanical behavior of beta-type titanium porous structures manufactured by electron beam melting and selective laser melting,” Acta Mater., vol. 113, pp. 56–67, 2016. [3] X. Wang, L. N. Carter, B. Pang, M. M. Attallah, and M. H. Loretto, “Microstructure and yield strength of SLM-fabricated {CM247LC} Ni-Superalloy,” Acta Mater., vol. 128, pp. 87–95, 2017. [4] R. Engeli, T. Etter, S. Hoevel, and K. Wegener, “Processability of different IN738LC powder batches by selective laser melting,” J. Mater. Process. Technol., vol. 229, pp. 484–491, 2016. [5] Haynes, “HAYNES ® 282 ® alloy,” 2017. [6] L. M. Pike, “Long term thermal exposure of Haynes 282 alloy,” Superalloy, vol. 718, pp. 644–660, 2010. [7] L. M. Pike, “HAYNES® 282TM Alloy: A New Wrought Superalloy Designed for Improved Creep Strength and Fabricability,” Processing, no. 42398, pp. 1031–1039, 2006. [8] S. K. Srivastava, J. L. Caron, and L. M. Pike, “Recent developments in the characteristics of Haynes 282 alloy for use in A-USC applications,” in Proceedings of the 7th International Conference, on Advances in Materials Technology for Fossil Power Plants, 2014, pp. 120–130. [9] J. N. DuPont, J. C. Lippold, and S. D. Kiser, Welding Metallurgy and Weldability of Nickel Base Alloys. 2009. [10] J. W. Brooks and P. J. Bridges, “Metallurgical stability of Inconel alloy 718,” Superalloys, vol. 88, pp. 33–42, 1988. [11] H.-E. Huang and C.-H. Koo, “Characteristics and mechanical properties of polycrystalline CM 247 LC superalloy casting,” Mater. Trans., vol. 45, no. 2, pp. 562–568, 2004. [12] K. L. Kruger, “HAYNES 282 alloy,” in Materials for ultra-supercritical and advanced ultra-supercritical power plants, Elsevier, 2017, pp. 511–545. [13] L. Wang et al., “Effect of heterogeneous microstructure on the tensile and creep performances of cast Haynes 282 alloy,” Mater. Sci. Eng. A, vol. 828, p. 142099, 2021. [14] L. O. Osoba and O. A. Ojo, “Influence of laser welding heat input on HAZ cracking in newly developed Haynes 282 superalloy Influence of laser welding heat input on HAZ cracking in newly developed Haynes 282 superalloy,” vol. 0836, no. May, 2012. [15] L. O. Osoba, R. G. Ding, and O. A. Ojo, “Improved resistance to laser weld heat-affected zone microfissuring in a newly developed superalloy HAYNES 282,” Metall. Mater. Trans. A, vol. 43, no. 11, pp. 4281–4295, 2012. [16] M. M. Kirka, K. A. Unocic, K. Kruger, and A. Forsythe, “Process Development for Haynes® 282® Using Additive Manufacturing,” Oak Ridge National Lab.(ORNL), Oak Ridge, TN (United States), 2018. [17] K. A. Unocic, M. M. Kirka, E. Cakmak, D. Greeley, A. O. Okello, and S. Dryepondt, “Evaluation of additive electron beam melting of haynes 282 alloy,” Mater. Sci. Eng. A, vol. 772, p. 138607, 2020. [18] A. Ramakrishnan and G. P. Dinda, “Microstructure and mechanical properties of direct laser metal deposited Haynes 282 superalloy,” Mater. Sci. Eng. A, vol. 748, pp. 347–356, 2019. [19] R. Otto, V. Brøtan, A. S. Azar, and O. Åsebø, “Processing of Haynes® 282® Alloy by Laser Powder Bed Fusion Technology,” in TMS 2019 148th Annual Meeting & Exhibition Supplemental Proceedings, 2019, pp. 503–510. [20] A. S. Shaikh, F. Schulz, K. Minet-Lallemand, and E. Hryha, “Microstructure and mechanical properties of Haynes 282 superalloy produced by laser powder bed fusion,” Mater. Today Commun., vol. 26, p. 102038, 2021. [21] K. A. Christofidou et al., “Microstructural control and optimization of Haynes 282 manufactured through laser powder bed fusion,” in Superalloys 2020, Springer, 2020, pp. 1014–1023. [22] J. Boswell, J. Jones, N. Barnard, D. Clark, M. Whittaker, and R. Lancaster, “The effects of energy density and heat treatment on the microstructure and mechanical properties of laser additive manufactured Haynes 282,” Mater. Des., vol. 205, p. 109725, 2021. [23] Steel University, “Solid Solution Strengthening.” [Online]. Available: https://steeluniversity.org/product/solid-solution-strengthening/. [Accessed: 25-Mar-2020]. [24] Y. Mishima, S. Ochiai, N. Hamao, M. Yodogawa, and T. Suzuki, “Solid solution hardening of nickel—role of transition metal and B-subgroup solutes—,” Trans. Japan Inst. Met., vol. 27, no. 9, pp. 656–664, 1986. [25] E. Nembach and G. Neite, “Precipitation hardening of superalloys by ordered γ′-particles,” Prog. Mater. Sci., vol. 29, no. 3, pp. 177–319, 1985. [26] B. Dubiel and J. Sieniawski, “Precipitates in Additively Manufactured Inconel 625 Superalloy,” Materials (Basel)., vol. 12, no. 7, p. 1144, 2019. [27] G. Marchese et al., “Influence of heat treatments on microstructure evolution and mechanical properties of Inconel 625 processed by laser powder bed fusion,” Mater. Sci. Eng. A, vol. 729, pp. 64–75, 2018. [28] A. J. Goodfellow et al., “Gamma prime precipitate evolution during aging of a model nickel-based superalloy,” Metall. Mater. Trans. A, vol. 49, no. 3, pp. 718–728, 2018. [29] X. Fan, Z. Guo, X. Wang, J. Yang, and J. Zou, “Morphology evolution of γ′ precipitates in a powder metallurgy Ni-base superalloy,” Mater. Charact., vol. 139, pp. 382–389, 2018. [30] G. P. Sabol and R. Stickler, “Microstructure of Nickel‐Based Superalloys,” Phys. status solidi, vol. 35, no. 1, pp. 11–52, 1969. [31] R. E. Smallman and A. H. W. Ngan, “Plastic deformation and dislocation behaviour,” Mod. Phys. Metall., pp. 357–414, 2014. [32] J. Humphreys, G. S. Rohrer, and A. Rollett, “Chapter 2 - The Deformed State,” J. Humphreys, G. S. Rohrer, and A. B. T.-R. and R. A. P. (Third E. Rollett, Eds. Oxford: Elsevier, 2017, pp. 13–79. [33] K. A. Rozman, “Characterization of high temperature fatigue mechanisms in Haynes 282 nickel based superalloy,” 2014. [34] T. Sourmail, P. Openacker, G. Hopkin, and H. Bhadeshia, “Annealing twins,” PPT] Phase Transform. complex Prop. Res. Gr. Univ. Cambridge. Retrieved from http//www. msm. cam. ac. uk/phasetrans/abstracts/annealing. twin. html. [35] W. C. Winegard, “Fundamentals of the solidification of metals,” Metall. Rev., vol. 6, no. 1, pp. 57–100, 1961. [36] W. Kurz and D. J. Fisher, Fundamentals of solidification. Trans Tech Publications, 1998. [37] D. R. Askeland, P. P. Fulay, and W. J. Wright, The Science and Engineering of Materials, SI Edition. Cengage Learning, 2011. [38] W. Kurz and R. Trivedi, “Rapid solidification processing and microstructure formation,” Mater. Sci. Eng. A, vol. 179, pp. 46–51, 1994. [39] C. Boig, “The application of additive manufacturing to nickel-base superalloys for turbocharger applications.” University of Sheffield, 2019. [40] N. J. Harrison, I. Todd, and K. Mumtaz, “Reduction of micro-cracking in nickel superalloys processed by Selective Laser Melting: A fundamental alloy design approach,” Acta Mater., vol. 94, pp. 59–68, 2015. [41] P. Tao, H. Li, B. Huang, Q. Hu, S. Gong, and Q. Xu, “The crystal growth, intercellular spacing and microsegregation of selective laser melted Inconel 718 superalloy,” Vacuum, vol. 159, pp. 382–390, 2019. [42] C. Hayzelden, J. J. Rayment, and B. Cantor, “Rapid solidification microstructures in austenitic Fe Ni alloys,” Acta Metall., vol. 31, no. 3, pp. 379–386, 1983. [43] N. A. Ahmad, A. A. Wheeler, W. J. Boettinger, and G. B. McFadden, “Solute trapping and solute drag in a phase-field model of rapid solidification,” Phys. Rev. E, vol. 58, no. 3, p. 3436, 1998. [44] M. Fousova, D. Dvorsky, M. Vronka, D. Vojtech, and P. Lejcek, “The use of selective laser melting to increase the performance of AlSi9Cu3Fe alloy,” Materials (Basel)., vol. 11, no. 10, p. 1918, 2018. [45] H. Davies, N. Shohoji, and D. Warrington, “The structures of rapidly quenched nickel-based superalloy ribbons produced by melt spinning,” in Rapidly Solidification and Technologies, 1980, pp. 153–164. [46] A. Popovich and V. Sufiiarov, “Metal powder additive manufacturing,” in New trends in 3D printing, IntechOpen, 2016. [47] C. Huang, T. Liu, X. Wang, C. Lu, D. Li, and Z. Lu, “Magnetic properties of nanocrystalline powder cores fabricated by mechanically crushed powders,” J. Iron Steel Res. Int., vol. 22, no. 1, pp. 67–71, 2015. [48] K. Riener et al., “Influence of particle size distribution and morphology on the properties of the powder feedstock as well as of AlSi10Mg parts produced by laser powder bed fusion (LPBF),” Addit. Manuf., vol. 34, p. 101286, 2020. [49] L. C. Ardila et al., “Effect of IN718 recycled powder reuse on properties of parts manufactured by means of selective laser melting,” Phys. Procedia, vol. 56, pp. 99–107, 2014. [50] N. L. Loh and K. Y. Sia, “An overview of hot isostatic pressing,” J. Mater. Process. Technol., vol. 30, no. 1, pp. 45–65, 1992. [51] W. T. Carter and M. G. Jones, “Direct Laser Sintering of Metals,” Proceeding SFF Symp., pp. 51–9, 1993. [52] C. W. Hull, “Apparatus for production of three-dimensional objects by stereolithography,” United States Patent, Appl., No. 638905, Filed, 1984. [53] K. Cooper, Rapid Prototyping Technology: Selection and Application. Taylor & Francis, 2001. [54] S. Mellor, L. Hao, and D. Zhang, “Additive manufacturing: A framework for implementation,” Int. J. Prod. Econ., vol. 149, pp. 194–201, 2014. [55] M. E. Lynch et al., “Design and topology/shape structural optimisation for additively manufactured cold sprayed components: This paper presents an additive manufactured cold spray component which is shape optimised to achieve 60% reduction in stress and 20% reduction in weigh,” Virtual Phys. Prototyp., vol. 8, no. 3, pp. 213–231, 2013. [56] N. Serres, D. Tidu, S. Sankare, and F. Hlawka, “Environmental comparison of MESO-CLAD® process and conventional machining implementing life cycle assessment,” J. Clean. Prod., vol. 19, no. 9–10, pp. 1117–1124, 2011. [57] D. S. Thomas and S. W. Gilbert, “Costs and cost effectiveness of additive manufacturing,” NIST Spec. Publ., vol. 1176, p. 12, 2014. [58] E. Atzeni and A. Salmi, “Economics of additive manufacturing for end-usable metal parts,” Int. J. Adv. Manuf. Technol., vol. 62, no. 9–12, pp. 1147–1155, 2012. [59] E. O. Olakanmi, R. F. Cochrane, and K. W. Dalgarno, “A review on selective laser sintering/melting (SLS/SLM) of aluminium alloy powders: Processing, microstructure, and properties,” Prog. Mater. Sci., vol. 74, pp. 401–477, 2015. [60] R. Otto et al., “Roadmap for additive manufacturing of HAYNES® 282® superalloy by laser beam powder bed fusion (PBF-LB) technology,” Mater. Des., vol. 204, p. 109656, 2021. [61] M. Vaezi, H. Seitz, and S. Yang, “A review on 3D micro-additive manufacturing technologies,” Int. J. Adv. Manuf. Technol., vol. 67, no. 5–8, pp. 1721–1754, 2013. [62] J. J. Lewandowski and M. Seifi, “Metal additive manufacturing: a review of mechanical properties,” Annu. Rev. Mater. Res., vol. 46, pp. 151–186, 2016. [63] W. E. King, A. T. Anderson, R. M. Ferencz, N. E. Hodge, and C. Kamath, “Laser powder bed fusion additive manufacturing of metals ; physics , computational , and materials challenges,” vol. 041304, no. 2015, 2017. [64] C. Y. Yap et al., “Review of selective laser melting: Materials and applications,” Appl. Phys. Rev., vol. 2, no. 4, p. 41101, 2015. [65] N. T. Aboulkhair, I. Maskery, C. Tuck, I. Ashcroft, and N. M. Everitt, “On the formation of AlSi10Mg single tracks and layers in selective laser melting: Microstructure and nano-mechanical properties,” J. Mater. Process. Technol., vol. 230, pp. 88–98, 2016. [66] T. Qi, H. Zhu, H. Zhang, J. Yin, L. Ke, and X. Zeng, “Selective laser melting of Al7050 powder: Melting mode transition and comparison of the characteristics between the keyhole and conduction mode,” Mater. Des., vol. 135, pp. 257–266, 2017. [67] S. M. Thompson, L. Bian, N. Shamsaei, and A. Yadollahi, “An overview of Direct Laser Deposition for additive manufacturing; Part I: Transport phenomena, modeling and diagnostics,” Addit. Manuf., vol. 8, pp. 36–62, 2015. [68] S. L. Sing, C. F. Tey, J. H. K. Tan, S. Huang, and W. Y. Yeong, “3D printing of metals in rapid prototyping of biomaterials: Techniques in additive manufacturing,” in Rapid prototyping of biomaterials, Elsevier, 2020, pp. 17–40. [69] A. J. Pinkerton, W. Wang, and L. Li, “Component repair using laser direct metal deposition,” Proc. Inst. Mech. Eng. Part B J. Eng. Manuf., vol. 222, no. 7, pp. 827–836, 2008. [70] K. Shah, I. ul Haq, A. Khan, S. A. Shah, M. Khan, and A. J. Pinkerton, “Parametric study of development of Inconel-steel functionally graded materials by laser direct metal deposition,” Mater. Des., vol. 54, pp. 531–538, 2014. [71] N. Shamsaei, A. Yadollahi, L. Bian, and S. M. Thompson, “An overview of Direct Laser Deposition for additive manufacturing; Part II: Mechanical behavior, process parameter optimization and control,” Addit. Manuf., vol. 8, pp. 12–35, 2015. [72] F. I. Azam, A. M. A. Rani, K. Altaf, T. Rao, and H. A. Zaharin, “An in-depth review on direct additive manufacturing of metals,” in IOP Conference Series: Materials Science and Engineering, 2018, vol. 328, no. 1, p. 12005. [73] F. Calignano et al., “Overview on additive manufacturing technologies,” Proc. IEEE, vol. 105, no. 4, pp. 593–612, 2017. [74] D. Deng, J. Moverare, R. L. Peng, and H. Söderberg, “Microstructure and anisotropic mechanical properties of EBM manufactured Inconel 718 and effects of post heat treatments,” Mater. Sci. Eng. A, vol. 693, pp. 151–163, 2017. [75] S. Moylan, J. Slotwinski, A. Cooke, K. Jurrens, and M. A. Donmez, “An additive manufacturing test artifact,” J. Res. Natl. Inst. Stand. Technol., vol. 119, p. 429, 2014. [76] K. J.P., W. X., L. T., and F. L., “Lasers and materials in selective laser sintering,” Assem. Autom., vol. 23, no. 4, pp. 357–371, Jan. 2003. [77] O. S. Fatoba, P. A. I. Popoola, S. L. Pityana, and O. S. Adesina, “Computational Dynamics of Anti-Corrosion Performance of Laser Alloyed Metallic Materials,” Fiber Laser, p. 345, 2016. [78] B. Wang and L. Gallais, “A theoretical investigation of the laser damage threshold of metal multi-dielectric mirrors for high power ultrashort applications,” Opt. Express, vol. 21, no. 12, pp. 14698–14711, 2013. [79] L. Caprio, A. G. Demir, and B. Previtali, “Influence of pulsed and continuous wave emission on melting efficiency in selective laser melting,” J. Mater. Process. Technol., vol. 266, pp. 429–441, 2019. [80] F. Freeman, “Structuring difference: the additive manufacture of spatially & functionally differentiated microstructures.” University of Sheffield, 2018. [81] A. G. Demir, P. Colombo, and B. Previtali, “From pulsed to continuous wave emission in SLM with contemporary fiber laser sources: effect of temporal and spatial pulse overlap in part quality,” Int. J. Adv. Manuf. Technol., vol. 91, no. 5–8, pp. 2701–2714, 2017. [82] A. Stwora and G. Skrabalak, “Influence of selected parameters of Selective Laser Sintering process on properties of sintered materials,” J. Achiev. Mater. Manuf. Eng., vol. 61, no. 2, pp. 375–380, 2013. [83] I. Koutiri, E. Pessard, P. Peyre, O. Amlou, and T. De Terris, “Influence of SLM process parameters on the surface finish, porosity rate and fatigue behavior of as-built Inconel 625 parts,” J. Mater. Process. Technol., vol. 255, pp. 536–546, 2018. [84] Y. M. Arısoy, L. E. Criales, T. Özel, B. Lane, S. Moylan, and A. Donmez, “Influence of scan strategy and process parameters on microstructure and its optimization in additively manufactured nickel alloy 625 via laser powder bed fusion,” Int. J. Adv. Manuf. Technol., vol. 90, no. 5–8, pp. 1393–1417, 2017. [85] J.-P. Kruth, L. Froyen, J. Van Vaerenbergh, P. Mercelis, M. Rombouts, and B. Lauwers, “Selective laser melting of iron-based powder,” J. Mater. Process. Technol., vol. 149, no. 1–3, pp. 616–622, 2004. [86] M. Thomas, G. J. Baxter, and I. Todd, “Normalised model-based processing diagrams for additive layer manufacture of engineering alloys,” Acta Mater., vol. 108, pp. 26–35, 2016. [87] A. Hilaire, E. Andrieu, and X. Wu, “High-temperature mechanical properties of alloy 718 produced by laser powder bed fusion with different processing parameters,” Addit. Manuf., vol. 26, pp. 147–160, 2019. [88] H. Hilal, R. Lancaster, S. Jeffs, J. Boswell, D. Stapleton, and G. Baxter, “The influence of process parameters and build orientation on the creep behaviour of a laser powder bed fused Ni-based superalloy for aerospace applications,” Materials (Basel)., vol. 12, no. 9, p. 1390, 2019. [89] W. E. King et al., “Observation of keyhole-mode laser melting in laser powder-bed fusion additive manufacturing,” J. Mater. Process. Technol., vol. 214, no. 12, pp. 2915–2925, 2014. [90] H. E. Helmer, C. Körner, and R. F. Singer, “Additive manufacturing of nickel-based superalloy Inconel 718 by selective electron beam melting: Processing window and microstructure,” J. Mater. Res., vol. 29, no. 17, pp. 1987–1996, 2014. [91] M. Dimter, R. Mayer, L. Hümmeler, R. Salzberger, J. Kotila, and T. Syvänen, “Method and device for manufacturing a three-dimensional object.” Google Patents, 11-Oct-2011. [92] K. Guan, Z. Wang, M. Gao, X. Li, and X. Zeng, “Effects of processing parameters on tensile properties of selective laser melted 304 stainless steel,” Mater. Des., vol. 50, pp. 581–586, 2013. [93] L. Thijs, F. Verhaeghe, T. Craeghs, J. Van Humbeeck, and J.-P. Kruth, “A study of the microstructural evolution during selective laser melting of Ti–6Al–4V,” Acta Mater., vol. 58, no. 9, pp. 3303–3312, 2010. [94] L. Thijs, M. L. M. Sistiaga, R. Wauthle, Q. Xie, J.-P. Kruth, and J. Van Humbeeck, “Strong morphological and crystallographic texture and resulting yield strength anisotropy in selective laser melted tantalum,” Acta Mater., vol. 61, no. 12, pp. 4657–4668, 2013. [95] P. Laakso et al., “Optimization and simulation of SLM process for high density H13 tool steel parts,” Phys. Procedia, vol. 83, pp. 26–35, 2016. [96] C. Panwisawas et al., “Keyhole formation and thermal fluid flow-induced porosity during laser fusion welding in titanium alloys: Experimental and modelling,” Acta Mater., vol. 126, pp. 251–263, 2017. [97] C. Qiu, C. Panwisawas, M. Ward, H. C. Basoalto, J. W. Brooks, and M. M. Attallah, “On the role of melt flow into the surface structure and porosity development during selective laser melting,” Acta Mater., vol. 96, pp. 72–79, 2015. [98] T. W. Eagar and N. S. Tsai, “Temperature fields produced by traveling distributed heat sources,” Weld. J., vol. 62, no. 12, pp. 346–355, 1983. [99] R. Snell et al., “Methods for Rapid Pore Classification in Metal Additive Manufacturing,” JOM, vol. 72, no. 1, pp. 101–109, 2020. [100] G. K. L. Ng, A. E. W. Jarfors, G. Bi, and H. Y. Zheng, “Porosity formation and gas bubble retention in laser metal deposition,” Appl. Phys. A, vol. 97, no. 3, p. 641, 2009. [101] H. L. Wei, J. W. Elmer, and T. DebRoy, “Crystal growth during keyhole mode laser welding,” Acta Mater., vol. 133, pp. 10–20, 2017. [102] H. L. Wei et al., “Mechanistic models for additive manufacturing of metallic components,” Prog. Mater. Sci., vol. 116, p. 100703, 2021. [103] M. B. Henderson, D. Arrell, R. Larsson, M. Heobel, and G. Marchant, “Nickel based superalloy welding practices for industrial gas turbine applications,” Sci. Technol. Weld. Join., vol. 9, no. 1, pp. 13–21, 2004. [104] L. N. Carter, M. M. Attallah, and R. C. Reed, “Laser powder bed fabrication of nickel-base superalloys: influence of parameters; characterisation, quantification and mitigation of cracking,” Superalloys, vol. 2012, pp. 577–586, 2012. [105] L. M. Pike, “Development of a fabricable gamma-prime (γ′) strengthened superalloy,” Superalloys 2008, pp. 191–200, 2008. [106] E. O. Hall and S. H. Algie, “The sigma phase,” Metall. Rev., vol. 11, no. 1, pp. 61–88, 1966. [107] X. Z. Qin, J. T. Guo, C. Yuan, G. X. Yang, L. Z. Zhou, and H. Q. Ye, “µ-Phase behavior in a cast Ni-base superalloy,” J. Mater. Sci., vol. 44, no. 18, pp. 4840–4847, 2009. [108] M. Morinaga, N. Yukawa, H. Adachi, and H. Ezaki, “New PHACOMP and its applications to alloy design,” Superalloys 1984, pp. 523–532, 1984. [109] K. Zhao, Y. H. Ma, and L. H. Lou, “Improvement of creep rupture strength of a liquid metal cooling directionally solidified nickel-base superalloy by carbides,” J. Alloys Compd., vol. 475, no. 1–2, pp. 648–651, 2009. [110] G. Cao and S. Kou, “Predicting and reducing liquation-cracking susceptibility based on temperature vs. fraction solid,” Weld. JOURNAL-NEW YORK-, vol. 85, no. 1, p. 9, 2006. [111] J. Zhang and R. F. Singer, “Hot tearing of nickel-based superalloys during directional solidification,” Acta Mater., vol. 50, no. 7, pp. 1869–1879, 2002. [112] M. Rappaz, J. Drezet, and M. Gremaud, “A New Hot-Tearing Criterion,” vol. 30, no. February, pp. 449–455, 1999. [113] K. L. S. Sharma, “6 - Automation Strategies,” K. L. S. B. T.-O. of I. P. A. (Second E. Sharma, Ed. Elsevier, 2017, pp. 53–74. [114] S.-H. Kim, Electric motor control: DC, AC, and BLDC motors. Elsevier, 2017. [115] J. G. Carbonell, R. S. Michalski, and T. M. Mitchell, “An overview of machine learning,” in Machine learning, Elsevier, 1983, pp. 3–23. [116] Y. Li, “Deep reinforcement learning: An overview,” arXiv Prepr. arXiv1701.07274, 2017. [117] I. Goodfellow et al., “cleverhans v0. 1: an adversarial machine learning library,” arXiv Prepr. arXiv1610.00768, vol. 1, 2016. [118] D. F. Specht, “Probabilistic neural networks,” Neural networks, vol. 3, no. 1, pp. 109–118, 1990. [119] J. S. Richman and J. R. Moorman, “Physiological time-series analysis using approximate entropy and sample entropy,” Am. J. Physiol. Circ. Physiol., vol. 278, no. 6, pp. H2039–H2049, 2000. [120] K. Lovegrove and W. Stein, Concentrating solar power technology: principles, developments and applications. Elsevier, 2012. [121] S. L. Wright, R. F. Marks, and W. I. Wang, “Reproducible temperature measurement of GaAs substrates during molecular beam epitaxial growth,” J. Vac. Sci. Technol. B Microelectron. Process. Phenom., vol. 4, no. 2, pp. 505–506, 1986. [122] Kleiber, “High speed pyrometer with fibre optics for very fast temperature mea- surements •.” [123] H. Watanabe, M. Susa, H. Fukuyama, and K. Nagata, “Phase dependence (liquid/solid) of normal spectral emissivities of noble metals at melting points,” Int. J. Thermophys., vol. 24, no. 1, pp. 223–237, 2003. [124] H. Watanabe, M. Susa, H. Fukuyama, and K. Nagata, “Phase (liquid/solid) dependence of the normal spectral emissivity for iron, cobalt, and nickel at melting points,” Int. J. Thermophys., vol. 24, no. 2, pp. 473–488, 2003. [125] Z. L. Kowalewski and A. Ustrzycka, “Creep deformation,” Encycl. Contin. Mech., pp. 499–508, 2020. [126] X. Song, L. Tang, Z. Chen, and R. Zhou, “Micro-mechanism during long-term creep of a precipitation-strengthened Ni-based superalloy,” J. Mater. Sci., vol. 52, no. 8, pp. 4587–4598, 2017. [127] Z. Chen et al., “Anisotropy of nickel-based superalloy K418 fabricated by selective laser melting,” Prog. Nat. Sci. Mater. Int., vol. 28, no. 4, pp. 496–504, 2018. [128] K. Kunze, T. Etter, J. Grässlin, and V. Shklover, “Texture, anisotropy in microstructure and mechanical properties of IN738LC alloy processed by selective laser melting (SLM),” Mater. Sci. Eng. A, vol. 620, pp. 213–222, 2015. [129] V. A. Popovich, E. V Borisov, V. Heurtebise, T. Riemslag, A. A. Popovich, and V. S. Sufiiarov, “Creep and Thermomechanical Fatigue of Functionally Graded Inconel 718 Produced by Additive Manufacturing BT - TMS 2018 147th Annual Meeting & Exhibition Supplemental Proceedings,” 2018, pp. 85–97. [130] F. T. Furillo, S. Purushothaman, and J. K. Tien, “Understanding the Larson-Miller parameter.[for extrapolating stress rupture and creep properties of steels and superalloys],” 1977. [131] B. Vrancken, L. Thijs, J.-P. Kruth, and J. Van Humbeeck, “Heat treatment of Ti6Al4V produced by Selective Laser Melting: Microstructure and mechanical properties,” J. Alloys Compd., vol. 541, pp. 177–185, 2012. [132] D. Deng, R. L. Peng, H. Brodin, and J. Moverare, “Microstructure and mechanical properties of Inconel 718 produced by selective laser melting: Sample orientation dependence and effects of post heat treatments,” Mater. Sci. Eng. A, vol. 713, pp. 294–306, 2018. [133] J. Schneider, B. Lund, and M. Fullen, “Effect of heat treatment variations on the mechanical properties of Inconel 718 selective laser melted specimens,” Addit. Manuf., vol. 21, pp. 248–254, 2018. [134] S. Raghavan et al., “Effect of different heat treatments on the microstructure and mechanical properties in selective laser melted INCONEL 718 alloy,” Mater. Manuf. Process., vol. 32, no. 14, pp. 1588–1595, 2017. [135] C. Joseph, C. Persson, and M. H. Colliander, “Influence of heat treatment on the microstructure and tensile properties of Ni-base superalloy Haynes 282,” Mater. Sci. Eng. A, vol. 679, pp. 520–530, 2017. [136] R. Ghiaasiaan, N. Ahmad, P. R. Gradl, S. Shao, and N. Shamsaei, “Additively manufactured Haynes 282: effect of unimodal vs. bimodal γʹ-microstructure on mechanical properties,” Mater. Sci. Eng. A, vol. 831, p. 142234, 2022. [137] S. Tammas-Williams, “Private Communications.” 2017. [138] A. Antonysamy, “Haynes 282 Heat Treatment.” 2018. [139] A. Antonysamy, “Private Communications.” 2020. [140] L. Osoba, “Microstructural analysis of laser weld fusion zone in Haynes 282 superalloy,” Mater. Charact., vol. 65, no. March, pp. 93–99, 2012. [141] D. A. Metzler, “Strain-age cracking susceptibility of Ni-based superalloys as a function of strain rate, temperature, and alloy composition,” Weld. J, vol. 91, no. 6, p. 64, 2012. [142] S. J. Foster et al., “Process-defect-structure-property correlations during laser powder bed fusion of alloy 718: role of in situ and ex situ characterizations,” Metall. Mater. Trans. A, vol. 49, no. 11, pp. 5775–5798, 2018. [143] M. Lamm and R. F. Singer, “The effect of casting conditions on the high-cycle fatigue properties of the single-crystal nickel-base superalloy PWA 1483,” Metall. Mater. Trans. A, vol. 38, no. 6, pp. 1177–1183, 2007. [144] N. Raghavan et al., “Localized melt-scan strategy for site specific control of grain size and primary dendrite arm spacing in electron beam additive manufacturing,” Acta Mater., vol. 140, pp. 375–387, 2017. [145] R. F. Brooks, A. P. Day, R. J. L. Andon, L. A. Chapman, K. C. Mills, and P. N. Quested, “Measurement of viscosities of metals and alloys with an oscillating viscometer,” High Temp. High Press., vol. 33, no. 1, pp. 73–82, 2001. [146] K. Eckler, D. M. Herlach, and M. J. Aziz, “Search for a solute-drag effect in dendritic solidification,” Acta Metall. Mater., vol. 42, no. 3, pp. 975–979, 1994. [147] R. N. Abdullaev, R. A. Khairulin, S. V Stankus, and Y. M. Kozlovskii, “Density and volumetric expansion of the Inconel 718 alloy in solid and liquid states,” Thermophys. Aeromechanics, vol. 26, no. 5, pp. 785–788, 2019. [148] A. Antonysamy, “Private Commuications.” . [149] B. Vandenbroucke and J.-P. Kruth, “Selective Laser Melting of Biocompatible Metals for Rapid,” Rapid Prototyp. J., vol. 13, no. 4, pp. 148–159, 2007. [150] Z. Wang, E. Denlinger, P. Michaleris, A. D. Stoica, D. Ma, and A. M. Beese, “Residual stress mapping in Inconel 625 fabricated through additive manufacturing: Method for neutron diffraction measurements to validate thermomechanical model predictions,” Mater. Des., vol. 113, pp. 169–177, 2017. [151] M. Mani, S. Feng, L. Brandon, A. Donmez, S. Moylan, and R. Fesperman, Measurement science needs for real-time control of additive manufacturing powder-bed fusion processes. CRC Press, 2017. [152] K. Chua, R. Calandra, R. McAllister, and S. Levine, “Deep reinforcement learning in a handful of trials using probabilistic dynamics models,” arXiv Prepr. arXiv1805.12114, 2018. [153] H. Bhadeshia, R. C. Dimitriu, S. Forsik, J. H. Pak, and J. H. Ryu, “Performance of neural networks in materials science,” Mater. Sci. Technol., vol. 25, no. 4, pp. 504–510, 2009. [154] W. H. Kruskal and W. A. Wallis, “Use of ranks in one-criterion variance analysis,” J. Am. Stat. Assoc., vol. 47, no. 260, pp. 583–621, 1952."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.878115"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/31413/1/Lyle%20-%202021-%20Optimising%20the%20Laser%20Powder%20Bed%20Fusion%20Process%20for%20the%20Manufacture%20of%20a%20Nickel%20Superalloy.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Laser Powder bed Fusion as a form of additive manufacturing is a potentially desirable method of manufacture for aircraft parts that use nickel superalloys. One of the barriers to greater adoption is the uncertainty in mechanical properties build quality and microstructure that can arise from the LPBF process. This project explores how this uncertainty can be reduced or eliminated. Different methods achieve this reduction in uncertainty. A method for characterising both the laser and scanner system is outlined and tested. The different melting modes that can occur between the laser and the material are investigated. A closed-loop control system that included a machine learning algorithm was successfully implemented. This control had a statistically significant effect on reducing the variation in thermal emissivities. Constraints found from experimental observations and fundamental physics were imposed to reduce the creation of defects. The mechanical performance of Haynes 282 was benchmarked against other manufacturing methods and other alloys to find that test samples built using LPBF performed as well as wrought or cast samples in elevated stress rupture testing. In order to improve mechanical properties such as high temperature stress rupture resistance, the susceptibility of Haynes 282 to different cracking mechanisms was investigated. This susceptibility was tested through models and analysis of the microstructure and cracks themselves. The susceptibility was tested at different beam velocities, and it was found that the thermal front velocity was found to be critical in influencing the likelihood of crack formation. When the results of these experiments are combined, it suggests parameter ranges that suit both the alloy and the machine, whilst the closed-loop control can stay within these ranges even when the geometry or process conditions vary. This project was funded by GKN Aerospace in conjunction with the Engineering and Physical Sciences Research Council (EPSRC)."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Optimising the Laser Powder Bed Fusion Process for the Manufacture of a Nickel Superalloy"]}]}],"canonical_facts":{"dc:contributor.advisor":["Iain, Todd","Katerina, Christofidou"],"dc:contributor.sponsor":["EPSRC"],"dc:creator":["Lyle, Alistair"],"dc:date":["2021-12"],"dc:date.issued":["2021-12"],"dc:description.abstract":["Laser Powder bed Fusion as a form of additive manufacturing is a potentially desirable method of manufacture for aircraft parts that use nickel superalloys. One of the barriers to greater adoption is the uncertainty in mechanical properties build quality and microstructure that can arise from the LPBF process. This project explores how this uncertainty can be reduced or eliminated. Different methods achieve this reduction in uncertainty. A method for characterising both the laser and scanner system is outlined and tested. The different melting modes that can occur between the laser and the material are investigated. A closed-loop control system that included a machine learning algorithm was successfully implemented. This control had a statistically significant effect on reducing the variation in thermal emissivities. Constraints found from experimental observations and fundamental physics were imposed to reduce the creation of defects. The mechanical performance of Haynes 282 was benchmarked against other manufacturing methods and other alloys to find that test samples built using LPBF performed as well as wrought or cast samples in elevated stress rupture testing. In order to improve mechanical properties such as high temperature stress rupture resistance, the susceptibility of Haynes 282 to different cracking mechanisms was investigated. This susceptibility was tested through models and analysis of the microstructure and cracks themselves. The susceptibility was tested at different beam velocities, and it was found that the thermal front velocity was found to be critical in influencing the likelihood of crack formation. When the results of these experiments are combined, it suggests parameter ranges that suit both the alloy and the machine, whilst the closed-loop control can stay within these ranges even when the geometry or process conditions vary. This project was funded by GKN Aerospace in conjunction with the Engineering and Physical Sciences Research Council (EPSRC)."],"dc:format":["text"],"dc:identifier":["uk.bl.ethos.878115"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/31413/1/Lyle%20-%202021-%20Optimising%20the%20Laser%20Powder%20Bed%20Fusion%20Process%20for%20the%20Manufacture%20of%20a%20Nickel%20Superalloy.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Materials Science and Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/31413/"],"dc:relation.references":["[1] C. T. Sims, “A history of superalloy metallurgy for superalloy metallurgists,” Superalloys, vol. 1984, pp. 399–419, 1984. [2] Y. J. Liu et al., “Microstructure, defects and mechanical behavior of beta-type titanium porous structures manufactured by electron beam melting and selective laser melting,” Acta Mater., vol. 113, pp. 56–67, 2016. [3] X. Wang, L. N. Carter, B. Pang, M. M. Attallah, and M. H. Loretto, “Microstructure and yield strength of SLM-fabricated {CM247LC} Ni-Superalloy,” Acta Mater., vol. 128, pp. 87–95, 2017. [4] R. Engeli, T. Etter, S. Hoevel, and K. Wegener, “Processability of different IN738LC powder batches by selective laser melting,” J. Mater. Process. Technol., vol. 229, pp. 484–491, 2016. [5] Haynes, “HAYNES ® 282 ® alloy,” 2017. [6] L. M. Pike, “Long term thermal exposure of Haynes 282 alloy,” Superalloy, vol. 718, pp. 644–660, 2010. [7] L. M. Pike, “HAYNES® 282TM Alloy: A New Wrought Superalloy Designed for Improved Creep Strength and Fabricability,” Processing, no. 42398, pp. 1031–1039, 2006. [8] S. K. Srivastava, J. L. Caron, and L. M. Pike, “Recent developments in the characteristics of Haynes 282 alloy for use in A-USC applications,” in Proceedings of the 7th International Conference, on Advances in Materials Technology for Fossil Power Plants, 2014, pp. 120–130. [9] J. N. DuPont, J. C. Lippold, and S. D. Kiser, Welding Metallurgy and Weldability of Nickel Base Alloys. 2009. [10] J. W. Brooks and P. J. Bridges, “Metallurgical stability of Inconel alloy 718,” Superalloys, vol. 88, pp. 33–42, 1988. [11] H.-E. Huang and C.-H. Koo, “Characteristics and mechanical properties of polycrystalline CM 247 LC superalloy casting,” Mater. Trans., vol. 45, no. 2, pp. 562–568, 2004. [12] K. L. Kruger, “HAYNES 282 alloy,” in Materials for ultra-supercritical and advanced ultra-supercritical power plants, Elsevier, 2017, pp. 511–545. [13] L. Wang et al., “Effect of heterogeneous microstructure on the tensile and creep performances of cast Haynes 282 alloy,” Mater. Sci. Eng. A, vol. 828, p. 142099, 2021. [14] L. O. Osoba and O. A. Ojo, “Influence of laser welding heat input on HAZ cracking in newly developed Haynes 282 superalloy Influence of laser welding heat input on HAZ cracking in newly developed Haynes 282 superalloy,” vol. 0836, no. May, 2012. [15] L. O. Osoba, R. G. Ding, and O. A. Ojo, “Improved resistance to laser weld heat-affected zone microfissuring in a newly developed superalloy HAYNES 282,” Metall. Mater. Trans. A, vol. 43, no. 11, pp. 4281–4295, 2012. [16] M. M. Kirka, K. A. Unocic, K. Kruger, and A. Forsythe, “Process Development for Haynes® 282® Using Additive Manufacturing,” Oak Ridge National Lab.(ORNL), Oak Ridge, TN (United States), 2018. [17] K. A. Unocic, M. M. Kirka, E. Cakmak, D. Greeley, A. O. Okello, and S. Dryepondt, “Evaluation of additive electron beam melting of haynes 282 alloy,” Mater. Sci. Eng. A, vol. 772, p. 138607, 2020. [18] A. Ramakrishnan and G. P. Dinda, “Microstructure and mechanical properties of direct laser metal deposited Haynes 282 superalloy,” Mater. Sci. Eng. A, vol. 748, pp. 347–356, 2019. [19] R. Otto, V. Brøtan, A. S. Azar, and O. Åsebø, “Processing of Haynes® 282® Alloy by Laser Powder Bed Fusion Technology,” in TMS 2019 148th Annual Meeting & Exhibition Supplemental Proceedings, 2019, pp. 503–510. [20] A. S. Shaikh, F. Schulz, K. Minet-Lallemand, and E. Hryha, “Microstructure and mechanical properties of Haynes 282 superalloy produced by laser powder bed fusion,” Mater. Today Commun., vol. 26, p. 102038, 2021. [21] K. A. Christofidou et al., “Microstructural control and optimization of Haynes 282 manufactured through laser powder bed fusion,” in Superalloys 2020, Springer, 2020, pp. 1014–1023. [22] J. Boswell, J. Jones, N. Barnard, D. Clark, M. Whittaker, and R. Lancaster, “The effects of energy density and heat treatment on the microstructure and mechanical properties of laser additive manufactured Haynes 282,” Mater. Des., vol. 205, p. 109725, 2021. [23] Steel University, “Solid Solution Strengthening.” [Online]. Available: https://steeluniversity.org/product/solid-solution-strengthening/. [Accessed: 25-Mar-2020]. [24] Y. Mishima, S. Ochiai, N. Hamao, M. Yodogawa, and T. Suzuki, “Solid solution hardening of nickel—role of transition metal and B-subgroup solutes—,” Trans. Japan Inst. Met., vol. 27, no. 9, pp. 656–664, 1986. [25] E. Nembach and G. Neite, “Precipitation hardening of superalloys by ordered γ′-particles,” Prog. Mater. Sci., vol. 29, no. 3, pp. 177–319, 1985. [26] B. Dubiel and J. Sieniawski, “Precipitates in Additively Manufactured Inconel 625 Superalloy,” Materials (Basel)., vol. 12, no. 7, p. 1144, 2019. [27] G. Marchese et al., “Influence of heat treatments on microstructure evolution and mechanical properties of Inconel 625 processed by laser powder bed fusion,” Mater. Sci. Eng. A, vol. 729, pp. 64–75, 2018. [28] A. J. Goodfellow et al., “Gamma prime precipitate evolution during aging of a model nickel-based superalloy,” Metall. Mater. Trans. A, vol. 49, no. 3, pp. 718–728, 2018. [29] X. Fan, Z. Guo, X. Wang, J. Yang, and J. Zou, “Morphology evolution of γ′ precipitates in a powder metallurgy Ni-base superalloy,” Mater. Charact., vol. 139, pp. 382–389, 2018. [30] G. P. Sabol and R. Stickler, “Microstructure of Nickel‐Based Superalloys,” Phys. status solidi, vol. 35, no. 1, pp. 11–52, 1969. [31] R. E. Smallman and A. H. W. Ngan, “Plastic deformation and dislocation behaviour,” Mod. Phys. Metall., pp. 357–414, 2014. [32] J. Humphreys, G. S. Rohrer, and A. Rollett, “Chapter 2 - The Deformed State,” J. Humphreys, G. S. Rohrer, and A. B. T.-R. and R. A. P. (Third E. Rollett, Eds. Oxford: Elsevier, 2017, pp. 13–79. [33] K. A. Rozman, “Characterization of high temperature fatigue mechanisms in Haynes 282 nickel based superalloy,” 2014. [34] T. Sourmail, P. Openacker, G. Hopkin, and H. Bhadeshia, “Annealing twins,” PPT] Phase Transform. complex Prop. Res. Gr. Univ. Cambridge. Retrieved from http//www. msm. cam. ac. uk/phasetrans/abstracts/annealing. twin. html. [35] W. C. Winegard, “Fundamentals of the solidification of metals,” Metall. Rev., vol. 6, no. 1, pp. 57–100, 1961. [36] W. Kurz and D. J. Fisher, Fundamentals of solidification. Trans Tech Publications, 1998. [37] D. R. Askeland, P. P. Fulay, and W. J. Wright, The Science and Engineering of Materials, SI Edition. Cengage Learning, 2011. [38] W. Kurz and R. Trivedi, “Rapid solidification processing and microstructure formation,” Mater. Sci. Eng. A, vol. 179, pp. 46–51, 1994. [39] C. Boig, “The application of additive manufacturing to nickel-base superalloys for turbocharger applications.” University of Sheffield, 2019. [40] N. J. Harrison, I. Todd, and K. Mumtaz, “Reduction of micro-cracking in nickel superalloys processed by Selective Laser Melting: A fundamental alloy design approach,” Acta Mater., vol. 94, pp. 59–68, 2015. [41] P. Tao, H. Li, B. Huang, Q. Hu, S. Gong, and Q. Xu, “The crystal growth, intercellular spacing and microsegregation of selective laser melted Inconel 718 superalloy,” Vacuum, vol. 159, pp. 382–390, 2019. [42] C. Hayzelden, J. J. Rayment, and B. Cantor, “Rapid solidification microstructures in austenitic Fe Ni alloys,” Acta Metall., vol. 31, no. 3, pp. 379–386, 1983. [43] N. A. Ahmad, A. A. Wheeler, W. J. Boettinger, and G. B. McFadden, “Solute trapping and solute drag in a phase-field model of rapid solidification,” Phys. Rev. E, vol. 58, no. 3, p. 3436, 1998. [44] M. Fousova, D. Dvorsky, M. Vronka, D. Vojtech, and P. Lejcek, “The use of selective laser melting to increase the performance of AlSi9Cu3Fe alloy,” Materials (Basel)., vol. 11, no. 10, p. 1918, 2018. [45] H. Davies, N. Shohoji, and D. Warrington, “The structures of rapidly quenched nickel-based superalloy ribbons produced by melt spinning,” in Rapidly Solidification and Technologies, 1980, pp. 153–164. [46] A. Popovich and V. Sufiiarov, “Metal powder additive manufacturing,” in New trends in 3D printing, IntechOpen, 2016. [47] C. Huang, T. Liu, X. Wang, C. Lu, D. Li, and Z. Lu, “Magnetic properties of nanocrystalline powder cores fabricated by mechanically crushed powders,” J. Iron Steel Res. Int., vol. 22, no. 1, pp. 67–71, 2015. [48] K. Riener et al., “Influence of particle size distribution and morphology on the properties of the powder feedstock as well as of AlSi10Mg parts produced by laser powder bed fusion (LPBF),” Addit. Manuf., vol. 34, p. 101286, 2020. [49] L. C. Ardila et al., “Effect of IN718 recycled powder reuse on properties of parts manufactured by means of selective laser melting,” Phys. Procedia, vol. 56, pp. 99–107, 2014. [50] N. L. Loh and K. Y. Sia, “An overview of hot isostatic pressing,” J. Mater. Process. Technol., vol. 30, no. 1, pp. 45–65, 1992. [51] W. T. Carter and M. G. Jones, “Direct Laser Sintering of Metals,” Proceeding SFF Symp., pp. 51–9, 1993. [52] C. W. Hull, “Apparatus for production of three-dimensional objects by stereolithography,” United States Patent, Appl., No. 638905, Filed, 1984. [53] K. Cooper, Rapid Prototyping Technology: Selection and Application. Taylor & Francis, 2001. [54] S. Mellor, L. Hao, and D. Zhang, “Additive manufacturing: A framework for implementation,” Int. J. Prod. Econ., vol. 149, pp. 194–201, 2014. [55] M. E. Lynch et al., “Design and topology/shape structural optimisation for additively manufactured cold sprayed components: This paper presents an additive manufactured cold spray component which is shape optimised to achieve 60% reduction in stress and 20% reduction in weigh,” Virtual Phys. Prototyp., vol. 8, no. 3, pp. 213–231, 2013. [56] N. Serres, D. Tidu, S. Sankare, and F. Hlawka, “Environmental comparison of MESO-CLAD® process and conventional machining implementing life cycle assessment,” J. Clean. Prod., vol. 19, no. 9–10, pp. 1117–1124, 2011. [57] D. S. Thomas and S. W. Gilbert, “Costs and cost effectiveness of additive manufacturing,” NIST Spec. Publ., vol. 1176, p. 12, 2014. [58] E. Atzeni and A. Salmi, “Economics of additive manufacturing for end-usable metal parts,” Int. J. Adv. Manuf. Technol., vol. 62, no. 9–12, pp. 1147–1155, 2012. [59] E. O. Olakanmi, R. F. Cochrane, and K. W. Dalgarno, “A review on selective laser sintering/melting (SLS/SLM) of aluminium alloy powders: Processing, microstructure, and properties,” Prog. Mater. Sci., vol. 74, pp. 401–477, 2015. [60] R. Otto et al., “Roadmap for additive manufacturing of HAYNES® 282® superalloy by laser beam powder bed fusion (PBF-LB) technology,” Mater. Des., vol. 204, p. 109656, 2021. [61] M. Vaezi, H. Seitz, and S. Yang, “A review on 3D micro-additive manufacturing technologies,” Int. J. Adv. Manuf. Technol., vol. 67, no. 5–8, pp. 1721–1754, 2013. [62] J. J. Lewandowski and M. Seifi, “Metal additive manufacturing: a review of mechanical properties,” Annu. Rev. Mater. Res., vol. 46, pp. 151–186, 2016. [63] W. E. King, A. T. Anderson, R. M. Ferencz, N. E. Hodge, and C. Kamath, “Laser powder bed fusion additive manufacturing of metals ; physics , computational , and materials challenges,” vol. 041304, no. 2015, 2017. [64] C. Y. Yap et al., “Review of selective laser melting: Materials and applications,” Appl. Phys. Rev., vol. 2, no. 4, p. 41101, 2015. [65] N. T. Aboulkhair, I. Maskery, C. Tuck, I. Ashcroft, and N. M. Everitt, “On the formation of AlSi10Mg single tracks and layers in selective laser melting: Microstructure and nano-mechanical properties,” J. Mater. Process. Technol., vol. 230, pp. 88–98, 2016. [66] T. Qi, H. Zhu, H. Zhang, J. Yin, L. Ke, and X. Zeng, “Selective laser melting of Al7050 powder: Melting mode transition and comparison of the characteristics between the keyhole and conduction mode,” Mater. Des., vol. 135, pp. 257–266, 2017. [67] S. M. Thompson, L. Bian, N. Shamsaei, and A. Yadollahi, “An overview of Direct Laser Deposition for additive manufacturing; Part I: Transport phenomena, modeling and diagnostics,” Addit. Manuf., vol. 8, pp. 36–62, 2015. [68] S. L. Sing, C. F. Tey, J. H. K. Tan, S. Huang, and W. Y. Yeong, “3D printing of metals in rapid prototyping of biomaterials: Techniques in additive manufacturing,” in Rapid prototyping of biomaterials, Elsevier, 2020, pp. 17–40. [69] A. J. Pinkerton, W. Wang, and L. Li, “Component repair using laser direct metal deposition,” Proc. Inst. Mech. Eng. Part B J. Eng. Manuf., vol. 222, no. 7, pp. 827–836, 2008. [70] K. Shah, I. ul Haq, A. Khan, S. A. Shah, M. Khan, and A. J. Pinkerton, “Parametric study of development of Inconel-steel functionally graded materials by laser direct metal deposition,” Mater. Des., vol. 54, pp. 531–538, 2014. [71] N. Shamsaei, A. Yadollahi, L. Bian, and S. M. Thompson, “An overview of Direct Laser Deposition for additive manufacturing; Part II: Mechanical behavior, process parameter optimization and control,” Addit. Manuf., vol. 8, pp. 12–35, 2015. [72] F. I. Azam, A. M. A. Rani, K. Altaf, T. Rao, and H. A. Zaharin, “An in-depth review on direct additive manufacturing of metals,” in IOP Conference Series: Materials Science and Engineering, 2018, vol. 328, no. 1, p. 12005. [73] F. Calignano et al., “Overview on additive manufacturing technologies,” Proc. IEEE, vol. 105, no. 4, pp. 593–612, 2017. [74] D. Deng, J. Moverare, R. L. Peng, and H. Söderberg, “Microstructure and anisotropic mechanical properties of EBM manufactured Inconel 718 and effects of post heat treatments,” Mater. Sci. Eng. A, vol. 693, pp. 151–163, 2017. [75] S. Moylan, J. Slotwinski, A. Cooke, K. Jurrens, and M. A. Donmez, “An additive manufacturing test artifact,” J. Res. Natl. Inst. Stand. Technol., vol. 119, p. 429, 2014. [76] K. J.P., W. X., L. T., and F. L., “Lasers and materials in selective laser sintering,” Assem. Autom., vol. 23, no. 4, pp. 357–371, Jan. 2003. [77] O. S. Fatoba, P. A. I. Popoola, S. L. Pityana, and O. S. Adesina, “Computational Dynamics of Anti-Corrosion Performance of Laser Alloyed Metallic Materials,” Fiber Laser, p. 345, 2016. [78] B. Wang and L. Gallais, “A theoretical investigation of the laser damage threshold of metal multi-dielectric mirrors for high power ultrashort applications,” Opt. Express, vol. 21, no. 12, pp. 14698–14711, 2013. [79] L. Caprio, A. G. Demir, and B. Previtali, “Influence of pulsed and continuous wave emission on melting efficiency in selective laser melting,” J. Mater. Process. Technol., vol. 266, pp. 429–441, 2019. [80] F. Freeman, “Structuring difference: the additive manufacture of spatially & functionally differentiated microstructures.” University of Sheffield, 2018. [81] A. G. Demir, P. Colombo, and B. Previtali, “From pulsed to continuous wave emission in SLM with contemporary fiber laser sources: effect of temporal and spatial pulse overlap in part quality,” Int. J. Adv. Manuf. Technol., vol. 91, no. 5–8, pp. 2701–2714, 2017. [82] A. Stwora and G. Skrabalak, “Influence of selected parameters of Selective Laser Sintering process on properties of sintered materials,” J. Achiev. Mater. Manuf. Eng., vol. 61, no. 2, pp. 375–380, 2013. [83] I. Koutiri, E. Pessard, P. Peyre, O. Amlou, and T. De Terris, “Influence of SLM process parameters on the surface finish, porosity rate and fatigue behavior of as-built Inconel 625 parts,” J. Mater. Process. Technol., vol. 255, pp. 536–546, 2018. [84] Y. M. Arısoy, L. E. Criales, T. Özel, B. Lane, S. Moylan, and A. Donmez, “Influence of scan strategy and process parameters on microstructure and its optimization in additively manufactured nickel alloy 625 via laser powder bed fusion,” Int. J. Adv. Manuf. Technol., vol. 90, no. 5–8, pp. 1393–1417, 2017. [85] J.-P. Kruth, L. Froyen, J. Van Vaerenbergh, P. Mercelis, M. Rombouts, and B. Lauwers, “Selective laser melting of iron-based powder,” J. Mater. Process. Technol., vol. 149, no. 1–3, pp. 616–622, 2004. [86] M. Thomas, G. J. Baxter, and I. Todd, “Normalised model-based processing diagrams for additive layer manufacture of engineering alloys,” Acta Mater., vol. 108, pp. 26–35, 2016. [87] A. Hilaire, E. Andrieu, and X. Wu, “High-temperature mechanical properties of alloy 718 produced by laser powder bed fusion with different processing parameters,” Addit. Manuf., vol. 26, pp. 147–160, 2019. [88] H. Hilal, R. Lancaster, S. Jeffs, J. Boswell, D. Stapleton, and G. Baxter, “The influence of process parameters and build orientation on the creep behaviour of a laser powder bed fused Ni-based superalloy for aerospace applications,” Materials (Basel)., vol. 12, no. 9, p. 1390, 2019. [89] W. E. King et al., “Observation of keyhole-mode laser melting in laser powder-bed fusion additive manufacturing,” J. Mater. Process. Technol., vol. 214, no. 12, pp. 2915–2925, 2014. [90] H. E. Helmer, C. Körner, and R. F. Singer, “Additive manufacturing of nickel-based superalloy Inconel 718 by selective electron beam melting: Processing window and microstructure,” J. Mater. Res., vol. 29, no. 17, pp. 1987–1996, 2014. [91] M. Dimter, R. Mayer, L. Hümmeler, R. Salzberger, J. Kotila, and T. Syvänen, “Method and device for manufacturing a three-dimensional object.” Google Patents, 11-Oct-2011. [92] K. Guan, Z. Wang, M. Gao, X. Li, and X. Zeng, “Effects of processing parameters on tensile properties of selective laser melted 304 stainless steel,” Mater. Des., vol. 50, pp. 581–586, 2013. [93] L. Thijs, F. Verhaeghe, T. Craeghs, J. Van Humbeeck, and J.-P. Kruth, “A study of the microstructural evolution during selective laser melting of Ti–6Al–4V,” Acta Mater., vol. 58, no. 9, pp. 3303–3312, 2010. [94] L. Thijs, M. L. M. Sistiaga, R. Wauthle, Q. Xie, J.-P. Kruth, and J. Van Humbeeck, “Strong morphological and crystallographic texture and resulting yield strength anisotropy in selective laser melted tantalum,” Acta Mater., vol. 61, no. 12, pp. 4657–4668, 2013. [95] P. Laakso et al., “Optimization and simulation of SLM process for high density H13 tool steel parts,” Phys. Procedia, vol. 83, pp. 26–35, 2016. [96] C. Panwisawas et al., “Keyhole formation and thermal fluid flow-induced porosity during laser fusion welding in titanium alloys: Experimental and modelling,” Acta Mater., vol. 126, pp. 251–263, 2017. [97] C. Qiu, C. Panwisawas, M. Ward, H. C. Basoalto, J. W. Brooks, and M. M. Attallah, “On the role of melt flow into the surface structure and porosity development during selective laser melting,” Acta Mater., vol. 96, pp. 72–79, 2015. [98] T. W. Eagar and N. S. Tsai, “Temperature fields produced by traveling distributed heat sources,” Weld. J., vol. 62, no. 12, pp. 346–355, 1983. [99] R. Snell et al., “Methods for Rapid Pore Classification in Metal Additive Manufacturing,” JOM, vol. 72, no. 1, pp. 101–109, 2020. [100] G. K. L. Ng, A. E. W. Jarfors, G. Bi, and H. Y. Zheng, “Porosity formation and gas bubble retention in laser metal deposition,” Appl. Phys. A, vol. 97, no. 3, p. 641, 2009. [101] H. L. Wei, J. W. Elmer, and T. DebRoy, “Crystal growth during keyhole mode laser welding,” Acta Mater., vol. 133, pp. 10–20, 2017. [102] H. L. Wei et al., “Mechanistic models for additive manufacturing of metallic components,” Prog. Mater. Sci., vol. 116, p. 100703, 2021. [103] M. B. Henderson, D. Arrell, R. Larsson, M. Heobel, and G. Marchant, “Nickel based superalloy welding practices for industrial gas turbine applications,” Sci. Technol. Weld. Join., vol. 9, no. 1, pp. 13–21, 2004. [104] L. N. Carter, M. M. Attallah, and R. C. Reed, “Laser powder bed fabrication of nickel-base superalloys: influence of parameters; characterisation, quantification and mitigation of cracking,” Superalloys, vol. 2012, pp. 577–586, 2012. [105] L. M. Pike, “Development of a fabricable gamma-prime (γ′) strengthened superalloy,” Superalloys 2008, pp. 191–200, 2008. [106] E. O. Hall and S. H. Algie, “The sigma phase,” Metall. Rev., vol. 11, no. 1, pp. 61–88, 1966. [107] X. Z. Qin, J. T. Guo, C. Yuan, G. X. Yang, L. Z. Zhou, and H. Q. Ye, “µ-Phase behavior in a cast Ni-base superalloy,” J. Mater. Sci., vol. 44, no. 18, pp. 4840–4847, 2009. [108] M. Morinaga, N. Yukawa, H. Adachi, and H. Ezaki, “New PHACOMP and its applications to alloy design,” Superalloys 1984, pp. 523–532, 1984. [109] K. Zhao, Y. H. Ma, and L. H. Lou, “Improvement of creep rupture strength of a liquid metal cooling directionally solidified nickel-base superalloy by carbides,” J. Alloys Compd., vol. 475, no. 1–2, pp. 648–651, 2009. [110] G. Cao and S. Kou, “Predicting and reducing liquation-cracking susceptibility based on temperature vs. fraction solid,” Weld. JOURNAL-NEW YORK-, vol. 85, no. 1, p. 9, 2006. [111] J. Zhang and R. F. Singer, “Hot tearing of nickel-based superalloys during directional solidification,” Acta Mater., vol. 50, no. 7, pp. 1869–1879, 2002. [112] M. Rappaz, J. Drezet, and M. Gremaud, “A New Hot-Tearing Criterion,” vol. 30, no. February, pp. 449–455, 1999. [113] K. L. S. Sharma, “6 - Automation Strategies,” K. L. S. B. T.-O. of I. P. A. (Second E. Sharma, Ed. Elsevier, 2017, pp. 53–74. [114] S.-H. Kim, Electric motor control: DC, AC, and BLDC motors. Elsevier, 2017. [115] J. G. Carbonell, R. S. Michalski, and T. M. Mitchell, “An overview of machine learning,” in Machine learning, Elsevier, 1983, pp. 3–23. [116] Y. Li, “Deep reinforcement learning: An overview,” arXiv Prepr. arXiv1701.07274, 2017. [117] I. Goodfellow et al., “cleverhans v0. 1: an adversarial machine learning library,” arXiv Prepr. arXiv1610.00768, vol. 1, 2016. [118] D. F. Specht, “Probabilistic neural networks,” Neural networks, vol. 3, no. 1, pp. 109–118, 1990. [119] J. S. Richman and J. R. Moorman, “Physiological time-series analysis using approximate entropy and sample entropy,” Am. J. Physiol. Circ. Physiol., vol. 278, no. 6, pp. H2039–H2049, 2000. [120] K. Lovegrove and W. Stein, Concentrating solar power technology: principles, developments and applications. Elsevier, 2012. [121] S. L. Wright, R. F. Marks, and W. I. Wang, “Reproducible temperature measurement of GaAs substrates during molecular beam epitaxial growth,” J. Vac. Sci. Technol. B Microelectron. Process. Phenom., vol. 4, no. 2, pp. 505–506, 1986. [122] Kleiber, “High speed pyrometer with fibre optics for very fast temperature mea- surements •.” [123] H. Watanabe, M. Susa, H. Fukuyama, and K. Nagata, “Phase dependence (liquid/solid) of normal spectral emissivities of noble metals at melting points,” Int. J. Thermophys., vol. 24, no. 1, pp. 223–237, 2003. [124] H. Watanabe, M. Susa, H. Fukuyama, and K. Nagata, “Phase (liquid/solid) dependence of the normal spectral emissivity for iron, cobalt, and nickel at melting points,” Int. J. Thermophys., vol. 24, no. 2, pp. 473–488, 2003. [125] Z. L. Kowalewski and A. Ustrzycka, “Creep deformation,” Encycl. Contin. Mech., pp. 499–508, 2020. [126] X. Song, L. Tang, Z. Chen, and R. Zhou, “Micro-mechanism during long-term creep of a precipitation-strengthened Ni-based superalloy,” J. Mater. Sci., vol. 52, no. 8, pp. 4587–4598, 2017. [127] Z. Chen et al., “Anisotropy of nickel-based superalloy K418 fabricated by selective laser melting,” Prog. Nat. Sci. Mater. Int., vol. 28, no. 4, pp. 496–504, 2018. [128] K. Kunze, T. Etter, J. Grässlin, and V. Shklover, “Texture, anisotropy in microstructure and mechanical properties of IN738LC alloy processed by selective laser melting (SLM),” Mater. Sci. Eng. A, vol. 620, pp. 213–222, 2015. [129] V. A. Popovich, E. V Borisov, V. Heurtebise, T. Riemslag, A. A. Popovich, and V. S. Sufiiarov, “Creep and Thermomechanical Fatigue of Functionally Graded Inconel 718 Produced by Additive Manufacturing BT - TMS 2018 147th Annual Meeting & Exhibition Supplemental Proceedings,” 2018, pp. 85–97. [130] F. T. Furillo, S. Purushothaman, and J. K. Tien, “Understanding the Larson-Miller parameter.[for extrapolating stress rupture and creep properties of steels and superalloys],” 1977. [131] B. Vrancken, L. Thijs, J.-P. Kruth, and J. Van Humbeeck, “Heat treatment of Ti6Al4V produced by Selective Laser Melting: Microstructure and mechanical properties,” J. Alloys Compd., vol. 541, pp. 177–185, 2012. [132] D. Deng, R. L. Peng, H. Brodin, and J. Moverare, “Microstructure and mechanical properties of Inconel 718 produced by selective laser melting: Sample orientation dependence and effects of post heat treatments,” Mater. Sci. Eng. A, vol. 713, pp. 294–306, 2018. [133] J. Schneider, B. Lund, and M. Fullen, “Effect of heat treatment variations on the mechanical properties of Inconel 718 selective laser melted specimens,” Addit. Manuf., vol. 21, pp. 248–254, 2018. [134] S. Raghavan et al., “Effect of different heat treatments on the microstructure and mechanical properties in selective laser melted INCONEL 718 alloy,” Mater. Manuf. Process., vol. 32, no. 14, pp. 1588–1595, 2017. [135] C. Joseph, C. Persson, and M. H. Colliander, “Influence of heat treatment on the microstructure and tensile properties of Ni-base superalloy Haynes 282,” Mater. Sci. Eng. A, vol. 679, pp. 520–530, 2017. [136] R. Ghiaasiaan, N. Ahmad, P. R. Gradl, S. Shao, and N. Shamsaei, “Additively manufactured Haynes 282: effect of unimodal vs. bimodal γʹ-microstructure on mechanical properties,” Mater. Sci. Eng. A, vol. 831, p. 142234, 2022. [137] S. Tammas-Williams, “Private Communications.” 2017. [138] A. Antonysamy, “Haynes 282 Heat Treatment.” 2018. [139] A. Antonysamy, “Private Communications.” 2020. [140] L. Osoba, “Microstructural analysis of laser weld fusion zone in Haynes 282 superalloy,” Mater. Charact., vol. 65, no. March, pp. 93–99, 2012. [141] D. A. Metzler, “Strain-age cracking susceptibility of Ni-based superalloys as a function of strain rate, temperature, and alloy composition,” Weld. J, vol. 91, no. 6, p. 64, 2012. [142] S. J. Foster et al., “Process-defect-structure-property correlations during laser powder bed fusion of alloy 718: role of in situ and ex situ characterizations,” Metall. Mater. Trans. A, vol. 49, no. 11, pp. 5775–5798, 2018. [143] M. Lamm and R. F. Singer, “The effect of casting conditions on the high-cycle fatigue properties of the single-crystal nickel-base superalloy PWA 1483,” Metall. Mater. Trans. A, vol. 38, no. 6, pp. 1177–1183, 2007. [144] N. Raghavan et al., “Localized melt-scan strategy for site specific control of grain size and primary dendrite arm spacing in electron beam additive manufacturing,” Acta Mater., vol. 140, pp. 375–387, 2017. [145] R. F. Brooks, A. P. Day, R. J. L. Andon, L. A. Chapman, K. C. Mills, and P. N. Quested, “Measurement of viscosities of metals and alloys with an oscillating viscometer,” High Temp. High Press., vol. 33, no. 1, pp. 73–82, 2001. [146] K. Eckler, D. M. Herlach, and M. J. Aziz, “Search for a solute-drag effect in dendritic solidification,” Acta Metall. Mater., vol. 42, no. 3, pp. 975–979, 1994. [147] R. N. Abdullaev, R. A. Khairulin, S. V Stankus, and Y. M. Kozlovskii, “Density and volumetric expansion of the Inconel 718 alloy in solid and liquid states,” Thermophys. Aeromechanics, vol. 26, no. 5, pp. 785–788, 2019. [148] A. Antonysamy, “Private Commuications.” . [149] B. Vandenbroucke and J.-P. Kruth, “Selective Laser Melting of Biocompatible Metals for Rapid,” Rapid Prototyp. J., vol. 13, no. 4, pp. 148–159, 2007. [150] Z. Wang, E. Denlinger, P. Michaleris, A. D. Stoica, D. Ma, and A. M. Beese, “Residual stress mapping in Inconel 625 fabricated through additive manufacturing: Method for neutron diffraction measurements to validate thermomechanical model predictions,” Mater. Des., vol. 113, pp. 169–177, 2017. [151] M. Mani, S. Feng, L. Brandon, A. Donmez, S. Moylan, and R. Fesperman, Measurement science needs for real-time control of additive manufacturing powder-bed fusion processes. CRC Press, 2017. [152] K. Chua, R. Calandra, R. McAllister, and S. Levine, “Deep reinforcement learning in a handful of trials using probabilistic dynamics models,” arXiv Prepr. arXiv1805.12114, 2018. [153] H. Bhadeshia, R. C. Dimitriu, S. Forsik, J. H. Pak, and J. H. Ryu, “Performance of neural networks in materials science,” Mater. Sci. Technol., vol. 25, no. 4, pp. 504–510, 2009. [154] W. H. Kruskal and W. A. Wallis, “Use of ranks in one-criterion variance analysis,” J. Am. Stat. Assoc., vol. 47, no. 260, pp. 583–621, 1952."],"dcterms:accessrights":["public"],"dc:title":["Optimising the Laser Powder Bed Fusion Process for the Manufacture of a Nickel Superalloy"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"],"person:identifier.orcid":["0000000316373525"]},"updated_at":"2026-11-18T23:19:31Z"}