{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:32595"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:32595","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Processing of NdFeB for Electric Motor Applications Using Selective Laser Melting","abstract":"The production of complex/intricate shaped NdFeB magnets can be challenging when using conventional manufacturing techniques due to their inherent brittle structure. The additive manufacturing technique selective laser melting (SLM) may offer an opportunity to produce NdFeB magnets with high geometric complexity and expand the range of applications and magnet capabilities. Nevertheless, some SLM processing challenges exist for the processing of this material, including the generation of the internal porosity due to the intermetallic structure of NdFeB, the creation of residual thermal stresses and crack formation due to the fast-cooling rate of the SLM process. The main objective of this work is to explore SLM process parameter effects on the formation of NdFeB, with the aim of reducing part porosity, internal cracks using process parameter optimization. This study for the first time will also explore the effect of using a heated powder during processing. In addition, this thesis is the first study which investigates the effect of heat treatment, Ni infiltration and HIPping on magnetic properties. During this investigation, it was found that low laser energy densities, between 50 to 100 J/mm3 enabled the fabrication of samples with up to 95.72 % density. Pores and crack defects were observed mainly on the edge of the samples. It was found that density is improved by lowering hatch distance and layer thickness, while the former has higher impact on sample density. Regarding the magnetic properties, magnets with a maximum energy product of 81 kJ/m3 could be produced without any post-treatment. Furthermore, there is no entirely linear relationship observed between the remanence and the density of the samples. Magnetic properties increase with the increasing volume fraction of the strong magnetic phase, Nd2Fe14B, in the samples. The density of the samples and remanence, Br can be improved with use of the heated bed while the coercivity, Hc decreases. The maximum energy product improved up to 84 kJ/m3. The Br improvement is related to density improvement, and Hc drops related to the bigger /or dendritic grains as a result of slowing cooling rates in heated bed. However, the integrity of the samples is less better than at room temperature fabrication. However, there is an improvement in the sample density, Br ,and Hc until 580 °C annealing temperature, then Hc starts to decrease while Br and density increases. The Br increment in heat treatment was not as expected according to the literature ofthe sintered magnets. It was found that Ni infiltration and HIPping did not improve the magnetic properties of the samples as the former was applied at very high temperatures (1400 °C), resulting in larger grains, reducing the coercivity. In addition, the amount of hard magnetic phase reduced after infiltration causing a reduction in Br.HIPping, causes loss of Nd rich phases with the application of heat and inert gas pressure on the samples during the process. Therefore, with the lack of isolating Nd rich grain boundaries, coercivity drops significantly. In summary, this study found that processing of NdFeB by SLM is very challenging. The brittle structure of the material with the combination of high cooling rates of the SLM, and the low strength of the material, makes it difficult to process without cracks and porosities. Additionally, the high oxygen sensitivity of the material compromises the phases for high magnetic properties, and the oxide layers on top of some samples make it difficult to get high-quality SEM images. However, the contributions of this study to literature are valuable. This study is the first which examines the effect of the heated bed. It was found that the heated bed has a potential to improve both the magnetic properties (remanence Br and maximum energy product BHmax) and the density of the magnets, in addition to improvement in surface quality. Also, it is the first study that examines the effect of heat treatment on magnetic properties. In addition, the relationship between the magnetic properties and printing parameters are valuable findings for literature. No other study in the literature discusses the Ф phase- a-Fe phase and printing parameter relationships. The SEM images and discussions are also valuable in an academic context since they clearly show the grain formation and morphology in the melt pool, and no discussion is found in the literature about them. Finally, the most important contribution is that the magnetic properties, Br and BHmax, are the highest properties that have improved so far, by parameter optimisation, without any post-processing or element doping, 0.72 T and 81 kJ/mm3, respectively.","abstract_html":"The production of complex/intricate shaped NdFeB magnets can be challenging when using conventional manufacturing techniques due to their inherent brittle structure. The additive manufacturing technique selective laser melting (SLM) may offer an opportunity to produce NdFeB magnets with high geometric complexity and expand the range of applications and magnet capabilities. Nevertheless, some SLM processing challenges exist for the processing of this material, including the generation of the internal porosity due to the intermetallic structure of NdFeB, the creation of residual thermal stresses and crack formation due to the fast-cooling rate of the SLM process. The main objective of this work is to explore SLM process parameter effects on the formation of NdFeB, with the aim of reducing part porosity, internal cracks using process parameter optimization. This study for the first time will also explore the effect of using a heated powder during processing. In addition, this thesis is the first study which investigates the effect of heat treatment, Ni infiltration and HIPping on magnetic properties. During this investigation, it was found that low laser energy densities, between 50 to 100 J/mm3 enabled the fabrication of samples with up to 95.72 % density. Pores and crack defects were observed mainly on the edge of the samples. It was found that density is improved by lowering hatch distance and layer thickness, while the former has higher impact on sample density. Regarding the magnetic properties, magnets with a maximum energy product of 81 kJ/m3 could be produced without any post-treatment. Furthermore, there is no entirely linear relationship observed between the remanence and the density of the samples. Magnetic properties increase with the increasing volume fraction of the strong magnetic phase, Nd2Fe14B, in the samples. The density of the samples and remanence, Br can be improved with use of the heated bed while the coercivity, Hc decreases. The maximum energy product improved up to 84 kJ/m3. The Br improvement is related to density improvement, and Hc drops related to the bigger /or dendritic grains as a result of slowing cooling rates in heated bed. However, the integrity of the samples is less better than at room temperature fabrication. However, there is an improvement in the sample density, Br ,and Hc until 580 °C annealing temperature, then Hc starts to decrease while Br and density increases. The Br increment in heat treatment was not as expected according to the literature ofthe sintered magnets. It was found that Ni infiltration and HIPping did not improve the magnetic properties of the samples as the former was applied at very high temperatures (1400 °C), resulting in larger grains, reducing the coercivity. In addition, the amount of hard magnetic phase reduced after infiltration causing a reduction in Br.HIPping, causes loss of Nd rich phases with the application of heat and inert gas pressure on the samples during the process. Therefore, with the lack of isolating Nd rich grain boundaries, coercivity drops significantly. In summary, this study found that processing of NdFeB by SLM is very challenging. The brittle structure of the material with the combination of high cooling rates of the SLM, and the low strength of the material, makes it difficult to process without cracks and porosities. Additionally, the high oxygen sensitivity of the material compromises the phases for high magnetic properties, and the oxide layers on top of some samples make it difficult to get high-quality SEM images. However, the contributions of this study to literature are valuable. This study is the first which examines the effect of the heated bed. It was found that the heated bed has a potential to improve both the magnetic properties (remanence Br and maximum energy product BHmax) and the density of the magnets, in addition to improvement in surface quality. Also, it is the first study that examines the effect of heat treatment on magnetic properties. In addition, the relationship between the magnetic properties and printing parameters are valuable findings for literature. No other study in the literature discusses the Ф phase- a-Fe phase and printing parameter relationships. The SEM images and discussions are also valuable in an academic context since they clearly show the grain formation and morphology in the melt pool, and no discussion is found in the literature about them. Finally, the most important contribution is that the magnetic properties, Br and BHmax, are the highest properties that have improved so far, by parameter optimisation, without any post-processing or element doping, 0.72 T and 81 kJ/mm3, respectively.","abstract_has_math":false,"creators":["Genc, Kubra"],"institution":"University of Sheffield","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Kamran, Mumtaz","Iain, Todd"],"committee_chairs":[],"committee_members":[],"year":2022,"date_issued":"2022-11","date_published":"2022-11","updated_at":"2026-11-18T23:22:02Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/32595/1/170276599%20Thesis%20Final%20Submission%20-corrected.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A32595","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Kamran, Mumtaz","Iain, Todd"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["Turkish Ministry of National Education","HiETA Technologies","Equipmake"]},{"key":"dc:creator","label":"Author","values":["Genc, Kubra"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2022-11"]},{"key":"dc:date.issued","label":"Date","values":["2022-11"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Mechanical Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/32595/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["References [1] K. Yamazaki and Y. Fukushima, “Effect of eddy-current loss reduction by magnet segmentation in synchronous motors with concentrated windings,” IEEE Trans Ind Appl, vol. 47, no. 2, pp. 779–788, 2011, doi: 10.1109/TIA.2010.2103915. [2] J. Jaćimović et al., “Net Shape 3D Printed NdFeB Permanent Magnet,” Adv Eng Mater, vol. 19, no. 8, pp. 1–7, 2017, doi: 10.1002/adem.201700098. [3] S. Amin, S. Madanzadeh, S. Khan, S. S. H. Bukhari, F. Akhtar, and J. S. Ro, “Effect of the magnet shape on the performance of coreless axial flux permanent magnet synchronous generator,” Electrical Engineering, vol. 104, no. 2, pp. 959–968, 2022, doi: 10.1007/s00202-021-01338-x. [4] J. Du, X. Wang, and H. Lv, “Optimization of Magnet Shape Based on Efficiency Map of IPMSM for EVs,” IEEE Transactions on Applied Superconductivity, vol. 26, no. 7, 2016, doi: 10.1109/TASC.2016.2594834. [5] M. Shokri, N. Rostami, V. Behjat, J. Pyrhonen, and M. Rostami, “Comparison of Performance Characteristics of Axial-Flux Permanent-Magnet Synchronous Machine with Different Magnet Shapes,” IEEE Trans Magn, vol. 51, no. 12, 2015, doi: 10.1109/TMAG.2015.2460217. [6] N. A. Spaldin, “Review of basic magnetostatics,” Magnetic Materials, pp. 3–13, 2012, doi: 10.1017/cbo9780511781599.001. [7] C. All, “_Units_and_Terminology_-_Magnetic_Materials_Group.pdf,” vol. 3, pp. 51–65. [8] N. A. Spaldin, “Magnetization and magnetic materials,” Magnetic Materials, pp. 14–21, 2012, doi: 10.1017/cbo9780511781599.002. [9] E. Wyslocka and R. Ulewicz, “Magnets: History, the Current State and the Future,” Metal 2015: 24Th International Conference on Metallurgy and Materials, no. July 2016, pp. 1680–1686, 2015. [10] M. J. Kramer, R. W. McCallum, I. A. Anderson, and S. Constantinides, “Prospects for non-rare earth permanent magnets for traction motors and generators,” Jom, vol. 64, no. 7, pp. 752–763, 2012, doi: 10.1007/s11837-012-0351-z. [11] H. Ferrites, S. Type, and N. Type, “Magnetic Materials : Hard Magnets,” pp. 1–8, 2010. [12] A. Williams, “Classification of Magnetic Materials,” Classification of Magnetic Materials, pp. 2–5, 2014, [Online]. Available: http://www.birmingham.ac.uk/research/activity/metallurgy-materials/magnets/Magnetic-Materials-Background-Information.aspx [13] S. et al. Kazawa, “‘Trends and Problems in Research of Permanent Magnets for Motors — Addressing Scarcity Problem of Rare Earth Elements —,’” Science & Technology Trends, no. 38, pp. 40–54, 2011. [14] I. S. Moosa, “History and Development of Permanent Magnets,” vol. 2, no. 1, pp. 18–26, 2014. [15] G. Bai, R. W. Gao, Y. Sun, G. B. Han, and B. Wang, “Study of high-coercivity sintered NdFeB magnets,” J Magn Magn Mater, vol. 308, no. 1, pp. 20–23, 2007, doi: 10.1016/j.jmmm.2006.04.029. [16] X. T. Tang, Z. W. Lu, and A. Z. Sun, “The effect of sintered Nd-Fe-B with Dy infiltration to the plating crafts,” J Magn Magn Mater, vol. 475, no. November 2018, pp. 10–13, 2019, doi: 10.1016/j.jmmm.2018.11.080. [17] X. G. Cui et al., “Magnetic properties and microstructure of sintered Nd–Fe–B magnets with intergranular addition of Ni powders,” J Alloys Compd, vol. 726, pp. 846–851, 2017, doi: 10.1016/j.jallcom.2017.08.061. [18] P. Zhang, L. Liang, J. Jin, Y. Zhang, X. Liu, and M. Yan, “Magnetic properties and corrosion resistance of Nd-Fe-B magnets with Nd64Co36intergranular addition,” J Alloys Compd, vol. 616, pp. 345–349, 2014, doi: 10.1016/j.jallcom.2014.07.085. [19] C. Jin et al., “Magnetic properties and phase evolution of sintered Nd-Fe-B magnets with intergranular addition of Pr–Co alloy,” J Alloys Compd, vol. 670, pp. 72–77, 2016, doi: 10.1016/j.jallcom.2016.02.006. [20] P. Zhang, T. Ma, L. Liang, and M. Yan, “Influence of Ta intergranular addition on microstructure and corrosion resistance of Nd-Dy-Fe-B sintered magnets,” J Alloys Compd, vol. 593, pp. 137–140, 2014, doi: 10.1016/j.jallcom.2014.01.055. [21] L. Li et al., “A novel method combining additive manufacturing and alloy infiltration for NdFeB bonded magnet fabrication,” J Magn Magn Mater, vol. 438, pp. 163–167, 2017, doi: 10.1016/j.jmmm.2017.04.066. [22] T. Sato, N. Oka, T. Ohsuna, Y. Kaneko, S. Suzuki, and T. Shima, “Enhancement of coercivity for Nd-Fe-B thin films by the infiltration of Nd-Cu alloy cap layer,” J Appl Phys, vol. 110, no. 2, pp. 1–5, 2011, doi: 10.1063/1.3608244. [23] W. Francis, “Definitions and Units,” Fuels and Fuel Technology, pp. 3–8, 2013, doi: 10.1016/b978-0-08-025250-6.50006-7. [24] T. Magnetic, “1 . 1 . 2 BASIC OPERATING PRINCIPLE OF ELECTRIC MOTORS,” no. 2017, pp. 56–58, 2023. [25] A. Hughes, Electric motors and drives [electronic resource] : fundamentals, types and applications, 3rd ed. Amsterdam ; Boston ; London: Elsevier Newnes, 2006. [26] A. E. Fitzgerald and S. D. Umans, Electric machinery, 6th ed. Boston, Mass. ; London: McGraw-Hill, 2003. [27] T. J. E. Miller, Brushless permanent-magnet and reluctance motor drives, 2nd (Corr.)impression. Oxford: Clarendon, 1993. [28] M. Šustek, M. Marcaník, P. Tomášek, and Z. Úředníček, “DC motors and servo-motors controlled by Raspberry Pi 2B,” MATEC Web of Conferences, vol. 125, pp. 1–6, 2017, doi: 10.1051/matecconf/201712502025. [29] J. R. Hendershot and T. J. E. Miller, Design of brushless permanent-magnet motors. Hillsboro, OH : Oxford: Magna Pysics Pub. ; Clarendon Press, 1994. [30] B. K. Bose, Modern power electronics and AC drives. Upper Saddle River, NJ: Prentice Hall PTR, 2002. [31] C. J. Fraser, “Electrical machines,” The Mechatronics Handbook, pp. 20-33-20–51, 2002, doi: 10.1201/9781420037043-13. [32] U. of LaSalle, “Magnetic Susceptibility,” Notes, no. May, pp. 4–7, 2014. [33] J. M. D. Coey, “Ferromagnetism and exchange,” in Magnetism and Magnetic Materials, 2010, pp. 128–129. doi: https://doi.org/10.1017/CBO9780511845000.006. [34] J. M. D. Coey, “Antiferromagnetism and other magnetic order,” in Magnetism and Magnetic Materials, 2010, pp. 195–230. doi: https://doi.org/10.1017/CBO9780511845000.007. [35] O. Fabiyi, “Chapter 3. Methodology,” Gated Neighbourhoods and privatisation of urban security in Ibadan Metropolis, pp. 27–29, 2016, doi: 10.4000/books.ifra.475. [36] E. P. Wohlfarth, “Hard magnetic materials,” Adv Phys, vol. 8, no. 30, pp. 87–224, 1959, doi: 10.1080/00018735900101178. [37] “6.9: Hard and Soft Magnets - Chemistry LibreTexts,” vol. 310, p. 189204, [Online]. Available: https://chem.libretexts.org/Bookshelves/Inorganic_Chemistry/Book%3A_Introduction_to_Inorganic_Chemistry/06%3A_Metals_and_Alloys-_Structure_Bonding_Electronic_and_Magnetic_Properties/6.09%3A_Hard_and_Soft_Magnets [38] H. R.Kirchmayr, “REVIEW ARTICLE Permanent magnets and hard magnetic materials,” J Appl Phys, vol. 29, pp. 2763–2778, 1996. [39] J. Karlsson and O. Söderström, “Review of Magnetic Materials Along With a Study of the Magnetic Stability and Solidity of Y40,” no. June, 2012, [Online]. Available: https://www.diva-portal.org/smash/get/diva2:534040/FULLTEXT01.pdf [40] L. H. Lewis and F. Jiménez-Villacorta, “Perspectives on permanent magnetic materials for energy conversion and power generation,” Metall Mater Trans A Phys Metall Mater Sci, vol. 44, no. SUPPL. 1, 2013, doi: 10.1007/s11661-012-1278-2. [41] eclipsemagnetics, “Magnet Materials & Assemblies - Sector Expertise - Power Generation.” https://www.eclipsemagnetics.com/row/magnet-materials-and-assemblies/?gclid=EAIaIQobChMI3q3V8ami4QIVGLLtCh2Klw_LEAAYASAAEgI_1_D_BwE [42] Sas.usace.army.mil., “Savannah District > About > Divisions and Offices > Operations Division > Richard B. Russell Dam and Lake > Hydropower > How Hydropower Works.” https://www.sas.usace.army.mil/About/Divisions-and-Offices/Operations-Division/Richard-B-Russell-Dam-and-Lake/Hydropower/ [43] H. Shokrollahi and K. Janghorban, “Soft magnetic composite materials (SMCs),” J Mater Process Technol, vol. 189, no. 1–3, pp. 1–12, 2007, doi: 10.1016/j.jmatprotec.2007.02.034. [44] J. E. Lenz, “A review of magnetic sensors,” Proceedings of the IEEE, vol. 78, no. 6, pp. 973–989, 1990. [45] McLaren Applied Technologies, “Permanent Magnet Alternator.” https://www.mclaren.com/appliedtechnologies/products/item/alternator-permanent-magnet/ [46] Adams Magnetic Products, “Magnets for Motor Applications.” https://www.adamsmagnetic.com/markets/magnets-motor-applications [47] Goudsmit, “Permanent Magnets and Precision Machined Parts for Medical Devices.” https://www.goudsmit.co.uk/sectors/medical/ [48] Q. A. Pankhurst, J. Connolly, S. K. Jones, and J. Dobson, “1110.J.Phys.D Appl.Phys.2003,36,R167.pdf,” vol. 36, 2003, doi: 10.1088/0022-3727/36/13/201. [49] M. A. Riley, A. D. Walmsley, J. D. Speight, and I. R. Harris, “Magnets in medicine,” Materials Science and Technology, vol. 18, no. 1, pp. 1–12, 2003, doi: 10.1179/026708301125000140. [50] A. du Plessis et al., “Standard method for microCT-based additive manufacturing quality control 2: Density measurement,” MethodsX, vol. 5, no. September, pp. 1117–1123, 2018, doi: 10.1016/j.mex.2018.09.006. [51] C. Rong and B. Shen, “Nanocrystalline and nanocomposite permanent magnets by melt spinning technique,” Chinese Physics B, vol. 27, no. 11, p. 117502, 2018, doi: 10.1088/1674-1056/27/11/117502. [52] B. J. F. Herbst, J. J. Croat, and F. E. Pinkerton, “Relationships Between Crystal Structure and Magnetic Properties in Nd 2 Fe 14 B,” no. April, 1984, doi: 10.1103/PhysRevB.29.4176. [53] K. Hono, “Strategy for high-coercivity Nd – Fe – B magnets,” Scr Mater, vol. 67, no. 6, pp. 530–535, 2012, doi: 10.1016/j.scriptamat.2012.06.038. [54] N. Magnets, “Mikrochimica Acta Metallurgical Factors Determining the Coercivity of,” pp. 115–124, 1987. [55] T. Shujian, L. Qingfan, L. Shixiang, and Z. Chaogui, “Phase diagram of the ternary system CeCl3-KCl-LiCl,” J Alloys Compd, vol. 274, no. 1–2, pp. 142–147, 1998, doi: 10.1016/S0925-8388(98)00551-9. [56] C. V. Mikler, V. Chaudhary, V. Soni, B. Gwalani, R. V. Ramanujan, and R. Banerjee, “Tuning the phase stability and magnetic properties of laser additively processed Fe-30at%Ni soft magnetic alloys,” Mater Lett, vol. 199, pp. 88–92, 2017, doi: 10.1016/j.matlet.2017.04.054. [57] X. Chen et al., “Laser additive processing of Fe-Si-B-Cu-Nb magnetic alloys,” J Manuf Process, vol. 29, pp. 175–181, 2017, doi: 10.1016/j.jmapro.2017.07.029. [58] C. V. Mikler et al., “Laser Additive Manufacturing of Magnetic Materials,” Jom, vol. 69, no. 3, pp. 532–543, 2017, doi: 10.1007/s11837-017-2257-2. [59] C. V. Mikler et al., “Laser additive processing of Ni-Fe-V and Ni-Fe-Mo Permalloys: Microstructure and magnetic properties,” Mater Lett, vol. 192, pp. 9–11, 2017, doi: 10.1016/j.matlet.2017.01.059. [60] B. Heer and A. Bandyopadhyay, “Compositionally graded magnetic-nonmagnetic bimetallic structure using laser engineered net shaping,” Mater Lett, vol. 216, pp. 16–19, 2018, doi: 10.1016/j.matlet.2017.12.129. [61] E. M. H. White, A. G. Kassen, E. Simsek, W. Tang, R. T. Ott, and I. E. Anderson, “Net Shape Processing of Alnico Magnets by Additive Manufacturing,” IEEE Trans Magn, vol. 53, no. 11, 2017, doi: 10.1109/TMAG.2017.2711965. [62] L. M. Bollig, P. J. Hilpisch, G. S. Mowry, and B. B. Nelson-Cheeseman, “3D printed magnetic polymer composite transformers,” J Magn Magn Mater, vol. 442, pp. 97–101, 2017, doi: 10.1016/j.jmmm.2017.06.070. [63] C. Huber et al., “3D print of polymer bonded rare-earth magnets, and 3D magnetic field scanning with an end-user 3D printer,” Appl Phys Lett, vol. 109, no. 16, 2016, doi: 10.1063/1.4964856. [64] S. J. Leigh, C. P. Purssell, D. R. Billson, and D. A. Hutchins, “Using a magnetite/thermoplastic composite in 3D printing of direct replacements for commercially available flow sensors,” Smart Mater Struct, vol. 23, no. 9, 2014, doi: 10.1088/0964-1726/23/9/095039. [65] L. Lu, P. Guo, and Y. Pan, “Magnetic-Field-Assisted Projection Stereolithography for Three-Dimensional Printing of Smart Structures,” J Manuf Sci Eng, vol. 139, no. 7, p. 071008, 2017, doi: 10.1115/1.4035964. [66] V. Popov, A. Koptyug, I. Radulov, F. Maccari, and G. Muller, “Prospects of additive manufacturing of rare-earth and non-rare-earth permanent magnets,” Procedia Manuf, vol. 21, no. 2017, pp. 100–108, 2018, doi: 10.1016/j.promfg.2018.02.199. [67] L. Li et al., “Big Area Additive Manufacturing of High Performance Bonded NdFeB Magnets,” Sci Rep, vol. 6, no. October, pp. 1–7, 2016, doi: 10.1038/srep36212. [68] L. Li, B. Post, V. Kunc, A. M. Elliott, and M. P. Paranthaman, “Additive manufacturing of near-net-shape bonded magnets: Prospects and challenges,” Scr Mater, vol. 135, pp. 100–104, 2017, doi: 10.1016/j.scriptamat.2016.12.035. [69] M. P. Paranthaman et al., “Binder Jetting : A Novel NdFeB Bonded Magnet Fabrication Process,” vol. 68, no. 7, pp. 1978–1982, 2016, doi: 10.1007/s11837-016-1883-4. [70] C. Vyas, G. Poologasundarampillai, J. Hoyland, and P. Bartolo, “12 - 3D printing of biocomposites for osteochondral tissue engineering,” in Biomedical Composites, 2017, pp. 261–302. doi: https://doi.org/10.1016/B978-0-08-100752-5.00013-5. [71] K. Anderson, C. Skelly, K. L. Martinson, K. L. Waite, P. M. Auwerda, and G. Heyboer, “Simultaneous multi-state equine business education program,” J Equine Vet Sci, vol. 33, no. 5, p. 389, 2013, doi: 10.1016/j.jevs.2013.03.154. [72] D. Herzog, V. Seyda, E. Wycisk, and C. Emmelmann, “Additive manufacturing of metals,” Acta Mater, vol. 117, pp. 371–392, 2016, doi: 10.1016/j.actamat.2016.07.019. [73] B. Zhang, N. E. Fenineche, L. Zhu, H. Liao, and C. Coddet, “Studies of magnetic properties of permalloy (Fe30%Ni) prepared by SLM technology,” J Magn Magn Mater, vol. 324, no. 4, pp. 495–500, 2012, doi: 10.1016/j.jmmm.2011.08.030. [74] B. Zhang, N. E. Fenineche, H. Liao, and C. Coddet, “Microstructure and magnetic properties of Fe-Ni alloy fabricated by selective laser melting Fe/Ni mixed powders,” J Mater Sci Technol, vol. 29, no. 8, pp. 757–760, 2013, doi: 10.1016/j.jmst.2013.05.001. [75] B. Zhang, N. E. Fenineche, H. Liao, and C. Coddet, “Magnetic properties of in-situ synthesized FeNi3 by selective laser melting Fe-80%Ni powders,” J Magn Magn Mater, vol. 336, pp. 49–54, 2013, doi: 10.1016/j.jmmm.2013.02.014. [76] T. Bauer, A. B. Spierings, and K. Wegener, “Microstructure and Electro-Magnetic Properties of a Nickel-Based Anti-Magnetic Shielding Alloy,” Proceedings of the 27th Annual International Solid Freeform Fabrication Symposium 2016, pp. 1856–1867, 2016. [77] K. J. Jhong, W. C. Huang, and W. H. Lee, “Microstructure and magnetic properties of magnetic material fabricated by selective laser melting,” Phys Procedia, vol. 83, pp. 818–824, 2016, doi: 10.1016/j.phpro.2016.08.084. [78] T. Kolb et al., “Laser Beam Melting of NdFeB for the production of rare-earth magnets,” 2016 6th International Electric Drives Production Conference, EDPC 2016 - Proceedings, pp. 34–40, 2016, doi: 10.1109/EDPC.2016.7851311. [79] N. Urban, F. Huber, and J. Franke, “Influences of process parameters on rare earth magnets produced by laser beam melting,” 2017 7th International Electric Drives Production Conference, EDPC 2017 - Proceedings, vol. 2017-Decem, pp. 1–5, 2018, doi: 10.1109/EDPC.2017.8328149. [80] D. Goll et al., “Refining the Microstructure of Fe-Nd-B by Selective Laser Melting,” Physica Status Solidi - Rapid Research Letters, vol. 13, no. 3, pp. 1–5, 2019, doi: 10.1002/pssr.201800536. [81] M. Skalon et al., “Influence of Melt-Pool Stability in 3D Printing of NdFeB Magnets on Density and Magnetic Properties,” Materials, vol. 13, no. 1, p. 139, 2019, doi: 10.3390/ma13010139. [82] D. Goll, F. Trauter, T. Bernthaler, J. Schanz, H. Riegel, and G. Schneider, “Additive manufacturing of bulk nanocrystalline fendb based permanent magnets,” Micromachines (Basel), vol. 12, no. 5, 2021, doi: 10.3390/mi12050538. [83] J. Wu, N. T. Aboulkhair, M. Degano, I. Ashcroft, and R. J. M. Hague, “Process-structure-property relationships in laser powder bed fusion of permanent magnetic Nd-Fe-B,” Mater Des, vol. 209, p. 109992, 2021, doi: 10.1016/j.matdes.2021.109992. [84] N. Urban, A. Meyer, S. Kreitlein, F. Leicht, and J. Franke, “Efficient near Net-Shape Production of High Energy Rare Earth Magnets by Laser Beam Melting,” Applied Mechanics and Materials, vol. 871, pp. 137–144, 2017, doi: 10.4028/www.scientific.net/amm.871.137. [85] F. Bittner, J. Thielsch, and W. G. Drossel, “Laser powder bed fusion of Nd–Fe–B permanent magnets,” Progress in Additive Manufacturing, vol. 5, no. 1, pp. 3–9, 2020, doi: 10.1007/s40964-020-00117-7. [86] F. Vial, F. Joly, E. Nevalainen, M. Sagawa, K. Hiraga, and K. T. Park, “Improvement of coercivity of sintered NdFeB permanent magnets by heat treatment,” J Magn Magn Mater, vol. 242–245, pp. 1329–1334, 2002, doi: 10.1016/S0304-8853(01)00967-2. [87] Y. Zhang et al., “Post-sinter annealing influences on coercivity of multi-main-phase Nd-Ce-Fe-B magnets,” Acta Mater, vol. 146, pp. 97–105, 2018, doi: 10.1016/j.actamat.2017.12.027. [88] N. Emminghaus, C. Hoff, J. Hermsdorf, and S. Kaierle, “Laser Powder Bed Fusion of NdFeB and influence of heat treatment on microstructure and crack development,” Procedia CIRP, vol. 94, pp. 211–216, 2020, doi: 10.1016/j.procir.2020.09.040. [89] H. R. Cha, K. W. Jeon, J. H. Yu, H. W. Kwon, Y. Do Kim, and J. G. Lee, “Coercivity enhancement of hot-deformed Nd-Fe-B magnet by grain boundary diffusion process using the reaction of NdHxand Cu nanopowders,” J Alloys Compd, vol. 693, pp. 744–748, 2017, doi: 10.1016/j.jallcom.2016.09.167. [90] M. Tang et al., “Microstructure modification and coercivity enhancement of Nd-Ce-Fe-B sintered magnets by grain boundary diffusing Nd-Dy-Al alloy,” J Magn Magn Mater, vol. 442, pp. 338–342, 2017, doi: 10.1016/j.jmmm.2017.06.116. [91] S. Guo, X. Zhang, G. Ding, R. Chen, D. Lee, and A. Yan, “Coercivity enhancement of sintered Nd-Fe-B magnets by chemical bath deposition of TbCl3,” J Appl Phys, vol. 115, no. 17, pp. 23–26, 2014, doi: 10.1063/1.4867962. [92] W. F. Li, T. Ohkubo, K. Hono, and M. Sagawa, “The origin of coercivity decrease in fine grained Nd-Fe-B sintered magnets,” J Magn Magn Mater, vol. 321, no. 8, pp. 1100–1105, 2009, doi: 10.1016/j.jmmm.2008.10.032. [93] H. W. Chang, Y. I. Lee, P. H. Liao, and W. C. Chang, “Significant coercivity enhancement of hot deformed NdFeB magnets by doping Ce-containing (PrNdCe)70Cu30 alloys powders,” Scr Mater, vol. 146, pp. 222–225, 2018, doi: 10.1016/j.scriptamat.2017.11.052. [94] X. Zheng et al., “Coercivity enhancement by inhibiting the formation of coarse grains region in hot-deformed Nd-Fe-B magnets with WC nano-particles addition,” Scr Mater, vol. 132, pp. 49–52, 2017, doi: 10.1016/j.scriptamat.2017.01.024. [95] X. Zhang et al., “Improvement of the thermal stability of sintered Nd-Fe-B magnets by intergranular addition of Dy82.3Co17.7,” J Appl Phys, vol. 115, no. 17, pp. 3–6, 2014, doi: 10.1063/1.4868491. [96] F. Bittner, J. Thielsch, and W. G. Drossel, “Microstructure and magnetic properties of Nd-Fe-B permanent magnets produced by laser powder bed fusion,” Scr Mater, vol. 201, p. 113921, 2021, doi: 10.1016/j.scriptamat.2021.113921. [97] S. Godavarthi, J. Porcayo-Calderon, E. Vazquez-Velez, M. Casales-Diaz, D. M. Ortega-Toledo, and L. Martinez-Gomez, “Influence of the chemical composition in the electrochemical response of permanent magnets,” Journal of Spectroscopy, vol. 2015, 2015, doi: 10.1155/2015/356027. [98] X. Y. Fang, D. Q. Yi, J. F. Nie, X. J. Zhang, B. Wang, and L. R. Xiao, “Effect of Zr, Mn and Sc additions on the grain size of Mg-Gd alloy,” J Alloys Compd, vol. 470, no. 1–2, pp. 311–316, 2009, doi: 10.1016/j.jallcom.2008.02.069. [99] H. W. Chang, C. H. Chiu, C. W. Chang, W. C. Chang, A. C. Sun, and Y. D. Yao, “Effect of Ti substitution on the magnetic properties, microstructure, and aftereffect of melt spun PrFeB nanocomposites,” Scr Mater, vol. 55, no. 6, pp. 529–532, 2006, doi: 10.1016/j.scriptamat.2006.05.032. [100] T. H. Coil, “Helmholtz coils Helmholtz coils,” no. 5. [101] LakeShore, “Measuring Permanent Magnet Characteristics with a Fluxmeter and Helmholtz Coil,” no. 614, 2010, [Online]. Available: www.lakeshore.com [102] T. Eb, “Chapter 4 Magnetic properties of the layer systems measured by SQUID magnetometry,” Measurement, pp. 27–40. [103] H. Gong, K. Rafi, H. Gu, T. Starr, and B. Stucker, “Analysis of defect generation in Ti-6Al-4V parts made using powder bed fusion additive manufacturing processes,” Addit Manuf, vol. 1, pp. 87–98, 2014, doi: 10.1016/j.addma.2014.08.002. [104] C. Chen, S. Chang, J. Zhu, Z. Xiao, H. Zhu, and X. Zeng, “Residual stress of typical parts in laser powder bed fusion,” J Manuf Process, vol. 59, no. October, pp. 621–628, 2020, doi: 10.1016/j.jmapro.2020.10.009. [105] E. Toyserkani et al., “Experimental and numerical investigation on the effect of layer thickness during laser powder-bed fusion of stainless steel 17-4PH,” International Journal of Rapid Manufacturing, vol. 9, no. 2/3, p. 1, 2020, doi: 10.1504/ijrapidm.2020.10029113. [106] X. Shi, C. Yan, W. Feng, Y. Zhang, and Z. Leng, “Effect of high layer thickness on surface quality and defect behavior of Ti-6Al-4V fabricated by selective laser melting,” Opt Laser Technol, vol. 132, no. June, p. 106471, 2020, doi: 10.1016/j.optlastec.2020.106471. [107] “White-paper1-EN”. [108] N. T. Oster, “Generation and characterization of anisotropic microstructures in rare earth-iron-boron alloys,” p. 134, 2012. [109] N. Sridharan et al., “Rationalization of solidification mechanism of Nd–Fe–B magnets during laser directed-energy deposition,” J Mater Sci, vol. 53, no. 11, pp. 8619–8626, 2018, doi: 10.1007/s10853-018-2178-7. [110] R. Li, Y. Shi, Z. Wang, L. Wang, J. Liu, and W. Jiang, “Densification behavior of gas and water atomized 316L stainless steel powder during selective laser melting,” Appl Surf Sci, vol. 256, no. 13, pp. 4350–4356, 2010, doi: 10.1016/j.apsusc.2010.02.030. [111] S. Waqar, K. Guo, and J. Sun, “Evolution of residual stress behavior in selective laser melting (SLM) of 316L stainless steel through preheating and in-situ re-scanning techniques,” Opt Laser Technol, vol. 149, no. June 2021, p. 107806, 2022, doi: 10.1016/j.optlastec.2021.107806. [112] M. M. Savalani and J. M. Pizarro, “Effect of preheat and layer thickness on selective laser melting (SLM) of magnesium,” Rapid Prototyp J, vol. 22, no. 1, pp. 115–122, 2016, doi: 10.1108/RPJ-07-2013-0076. [113] A. Mazilkin et al., “Grain boundary oxide layers in NdFeB-based permanent magnets,” Mater Des, vol. 199, p. 109417, 2021, doi: 10.1016/j.matdes.2020.109417. [114] T. de Terris et al., “Optimization and comparison of porosity rate measurement methods of Selective Laser Melted metallic parts,” Addit Manuf, vol. 28, no. May, pp. 802–813, 2019, doi: 10.1016/j.addma.2019.05.035. [115] M. Heydarzadeh Sohi, M. Ebrahimi, A. Honarbakhsh Raouf, and F. Mahboubi, “Comparative study of the corrosion behaviour of plasma nitrocarburised AISI4140 steel before and after post-oxidation,” Mater Des, vol. 31, no. 9, pp. 4432–4437, 2010, doi: 10.1016/j.matdes.2010.04.017. [116] C. Huber et al., “Coercivity enhancement of selective laser sintered NdFeB magnets by grain boundary infiltration,” Acta Mater, vol. 172, pp. 66–71, 2019, doi: 10.1016/j.actamat.2019.04.037. [117] A. S. Volegov et al., “Additive manufacturing of heavy rare earth free high-coercivity permanent magnets,” Acta Mater, vol. 188, pp. 733–739, 2020, doi: 10.1016/j.actamat.2020.02.058. [118] K. Essa, P. Jamshidi, J. Zou, M. M. Attallah, and H. Hassanin, “Porosity control in 316L stainless steel using cold and hot isostatic pressing,” Mater Des, vol. 138, pp. 21–29, 2018, doi: 10.1016/j.matdes.2017.10.025. [119] H. V. Atkinson and S. Davies, “Fundamental aspects of hot isostatic pressing: An overview,” Metall Mater Trans A Phys Metall Mater Sci, vol. 31, no. 12, pp. 2981–3000, 2000, doi: 10.1007/s11661-000-0078-2. [120] F. Yang et al., “Performance of Nd-Fe-B Magnets Fabricated by Hot Isostatic Pressing and Low-Temperature Sintering,” J Mater Eng Perform, vol. 28, no. 1, pp. 273–277, 2019, doi: 10.1007/s11665-018-3832-6. [121] Z. Q. Liao, F. Xu, W. J. Yan, Q. J. Huang, G. Chen, and S. D. Li, “Influence of cladless hot isostatic pressing on magnetic properties and corrosion resistance of sintered NdFeB magnets,” Key Eng Mater, vol. 538, pp. 211–214, 2013, doi: 10.4028/www.scientific.net/KEM.538.211. [122] J. Liu et al., “Grain size dependence of coercivity of hot-deformed Nd-Fe-B anisotropic magnets,” Acta Mater, vol. 82, pp. 336–343, 2015, doi: 10.1016/j.actamat.2014.09.021."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/32595/1/170276599%20Thesis%20Final%20Submission%20-corrected.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["The production of complex/intricate shaped NdFeB magnets can be challenging when using conventional manufacturing techniques due to their inherent brittle structure. The additive manufacturing technique selective laser melting (SLM) may offer an opportunity to produce NdFeB magnets with high geometric complexity and expand the range of applications and magnet capabilities. Nevertheless, some SLM processing challenges exist for the processing of this material, including the generation of the internal porosity due to the intermetallic structure of NdFeB, the creation of residual thermal stresses and crack formation due to the fast-cooling rate of the SLM process. The main objective of this work is to explore SLM process parameter effects on the formation of NdFeB, with the aim of reducing part porosity, internal cracks using process parameter optimization. This study for the first time will also explore the effect of using a heated powder during processing. In addition, this thesis is the first study which investigates the effect of heat treatment, Ni infiltration and HIPping on magnetic properties. During this investigation, it was found that low laser energy densities, between 50 to 100 J/mm3 enabled the fabrication of samples with up to 95.72 % density. Pores and crack defects were observed mainly on the edge of the samples. It was found that density is improved by lowering hatch distance and layer thickness, while the former has higher impact on sample density. Regarding the magnetic properties, magnets with a maximum energy product of 81 kJ/m3 could be produced without any post-treatment. Furthermore, there is no entirely linear relationship observed between the remanence and the density of the samples. Magnetic properties increase with the increasing volume fraction of the strong magnetic phase, Nd2Fe14B, in the samples. The density of the samples and remanence, Br can be improved with use of the heated bed while the coercivity, Hc decreases. The maximum energy product improved up to 84 kJ/m3. The Br improvement is related to density improvement, and Hc drops related to the bigger /or dendritic grains as a result of slowing cooling rates in heated bed. However, the integrity of the samples is less better than at room temperature fabrication. However, there is an improvement in the sample density, Br ,and Hc until 580 °C annealing temperature, then Hc starts to decrease while Br and density increases. The Br increment in heat treatment was not as expected according to the literature ofthe sintered magnets. It was found that Ni infiltration and HIPping did not improve the magnetic properties of the samples as the former was applied at very high temperatures (1400 °C), resulting in larger grains, reducing the coercivity. In addition, the amount of hard magnetic phase reduced after infiltration causing a reduction in Br.HIPping, causes loss of Nd rich phases with the application of heat and inert gas pressure on the samples during the process. Therefore, with the lack of isolating Nd rich grain boundaries, coercivity drops significantly. In summary, this study found that processing of NdFeB by SLM is very challenging. The brittle structure of the material with the combination of high cooling rates of the SLM, and the low strength of the material, makes it difficult to process without cracks and porosities. Additionally, the high oxygen sensitivity of the material compromises the phases for high magnetic properties, and the oxide layers on top of some samples make it difficult to get high-quality SEM images. However, the contributions of this study to literature are valuable. This study is the first which examines the effect of the heated bed. It was found that the heated bed has a potential to improve both the magnetic properties (remanence Br and maximum energy product BHmax) and the density of the magnets, in addition to improvement in surface quality. Also, it is the first study that examines the effect of heat treatment on magnetic properties. In addition, the relationship between the magnetic properties and printing parameters are valuable findings for literature. No other study in the literature discusses the Ф phase- a-Fe phase and printing parameter relationships. The SEM images and discussions are also valuable in an academic context since they clearly show the grain formation and morphology in the melt pool, and no discussion is found in the literature about them. Finally, the most important contribution is that the magnetic properties, Br and BHmax, are the highest properties that have improved so far, by parameter optimisation, without any post-processing or element doping, 0.72 T and 81 kJ/mm3, respectively."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Processing of NdFeB for Electric Motor Applications Using Selective Laser Melting"]}]}],"canonical_facts":{"dc:contributor.advisor":["Kamran, Mumtaz","Iain, Todd"],"dc:contributor.sponsor":["Turkish Ministry of National Education","HiETA Technologies","Equipmake"],"dc:creator":["Genc, Kubra"],"dc:date":["2022-11"],"dc:date.issued":["2022-11"],"dc:description.abstract":["The production of complex/intricate shaped NdFeB magnets can be challenging when using conventional manufacturing techniques due to their inherent brittle structure. The additive manufacturing technique selective laser melting (SLM) may offer an opportunity to produce NdFeB magnets with high geometric complexity and expand the range of applications and magnet capabilities. Nevertheless, some SLM processing challenges exist for the processing of this material, including the generation of the internal porosity due to the intermetallic structure of NdFeB, the creation of residual thermal stresses and crack formation due to the fast-cooling rate of the SLM process. The main objective of this work is to explore SLM process parameter effects on the formation of NdFeB, with the aim of reducing part porosity, internal cracks using process parameter optimization. This study for the first time will also explore the effect of using a heated powder during processing. In addition, this thesis is the first study which investigates the effect of heat treatment, Ni infiltration and HIPping on magnetic properties. During this investigation, it was found that low laser energy densities, between 50 to 100 J/mm3 enabled the fabrication of samples with up to 95.72 % density. Pores and crack defects were observed mainly on the edge of the samples. It was found that density is improved by lowering hatch distance and layer thickness, while the former has higher impact on sample density. Regarding the magnetic properties, magnets with a maximum energy product of 81 kJ/m3 could be produced without any post-treatment. Furthermore, there is no entirely linear relationship observed between the remanence and the density of the samples. Magnetic properties increase with the increasing volume fraction of the strong magnetic phase, Nd2Fe14B, in the samples. The density of the samples and remanence, Br can be improved with use of the heated bed while the coercivity, Hc decreases. The maximum energy product improved up to 84 kJ/m3. The Br improvement is related to density improvement, and Hc drops related to the bigger /or dendritic grains as a result of slowing cooling rates in heated bed. However, the integrity of the samples is less better than at room temperature fabrication. However, there is an improvement in the sample density, Br ,and Hc until 580 °C annealing temperature, then Hc starts to decrease while Br and density increases. The Br increment in heat treatment was not as expected according to the literature ofthe sintered magnets. It was found that Ni infiltration and HIPping did not improve the magnetic properties of the samples as the former was applied at very high temperatures (1400 °C), resulting in larger grains, reducing the coercivity. In addition, the amount of hard magnetic phase reduced after infiltration causing a reduction in Br.HIPping, causes loss of Nd rich phases with the application of heat and inert gas pressure on the samples during the process. Therefore, with the lack of isolating Nd rich grain boundaries, coercivity drops significantly. In summary, this study found that processing of NdFeB by SLM is very challenging. The brittle structure of the material with the combination of high cooling rates of the SLM, and the low strength of the material, makes it difficult to process without cracks and porosities. Additionally, the high oxygen sensitivity of the material compromises the phases for high magnetic properties, and the oxide layers on top of some samples make it difficult to get high-quality SEM images. However, the contributions of this study to literature are valuable. This study is the first which examines the effect of the heated bed. It was found that the heated bed has a potential to improve both the magnetic properties (remanence Br and maximum energy product BHmax) and the density of the magnets, in addition to improvement in surface quality. Also, it is the first study that examines the effect of heat treatment on magnetic properties. In addition, the relationship between the magnetic properties and printing parameters are valuable findings for literature. No other study in the literature discusses the Ф phase- a-Fe phase and printing parameter relationships. The SEM images and discussions are also valuable in an academic context since they clearly show the grain formation and morphology in the melt pool, and no discussion is found in the literature about them. Finally, the most important contribution is that the magnetic properties, Br and BHmax, are the highest properties that have improved so far, by parameter optimisation, without any post-processing or element doping, 0.72 T and 81 kJ/mm3, respectively."],"dc:format":["text"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/32595/1/170276599%20Thesis%20Final%20Submission%20-corrected.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Mechanical Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/32595/"],"dc:relation.references":["References [1] K. Yamazaki and Y. Fukushima, “Effect of eddy-current loss reduction by magnet segmentation in synchronous motors with concentrated windings,” IEEE Trans Ind Appl, vol. 47, no. 2, pp. 779–788, 2011, doi: 10.1109/TIA.2010.2103915. [2] J. Jaćimović et al., “Net Shape 3D Printed NdFeB Permanent Magnet,” Adv Eng Mater, vol. 19, no. 8, pp. 1–7, 2017, doi: 10.1002/adem.201700098. [3] S. Amin, S. Madanzadeh, S. Khan, S. S. H. Bukhari, F. Akhtar, and J. S. Ro, “Effect of the magnet shape on the performance of coreless axial flux permanent magnet synchronous generator,” Electrical Engineering, vol. 104, no. 2, pp. 959–968, 2022, doi: 10.1007/s00202-021-01338-x. [4] J. Du, X. Wang, and H. Lv, “Optimization of Magnet Shape Based on Efficiency Map of IPMSM for EVs,” IEEE Transactions on Applied Superconductivity, vol. 26, no. 7, 2016, doi: 10.1109/TASC.2016.2594834. [5] M. Shokri, N. Rostami, V. Behjat, J. Pyrhonen, and M. Rostami, “Comparison of Performance Characteristics of Axial-Flux Permanent-Magnet Synchronous Machine with Different Magnet Shapes,” IEEE Trans Magn, vol. 51, no. 12, 2015, doi: 10.1109/TMAG.2015.2460217. [6] N. A. Spaldin, “Review of basic magnetostatics,” Magnetic Materials, pp. 3–13, 2012, doi: 10.1017/cbo9780511781599.001. [7] C. All, “_Units_and_Terminology_-_Magnetic_Materials_Group.pdf,” vol. 3, pp. 51–65. [8] N. A. Spaldin, “Magnetization and magnetic materials,” Magnetic Materials, pp. 14–21, 2012, doi: 10.1017/cbo9780511781599.002. [9] E. Wyslocka and R. Ulewicz, “Magnets: History, the Current State and the Future,” Metal 2015: 24Th International Conference on Metallurgy and Materials, no. July 2016, pp. 1680–1686, 2015. [10] M. J. Kramer, R. W. McCallum, I. A. Anderson, and S. Constantinides, “Prospects for non-rare earth permanent magnets for traction motors and generators,” Jom, vol. 64, no. 7, pp. 752–763, 2012, doi: 10.1007/s11837-012-0351-z. [11] H. Ferrites, S. Type, and N. Type, “Magnetic Materials : Hard Magnets,” pp. 1–8, 2010. [12] A. Williams, “Classification of Magnetic Materials,” Classification of Magnetic Materials, pp. 2–5, 2014, [Online]. Available: http://www.birmingham.ac.uk/research/activity/metallurgy-materials/magnets/Magnetic-Materials-Background-Information.aspx [13] S. et al. Kazawa, “‘Trends and Problems in Research of Permanent Magnets for Motors — Addressing Scarcity Problem of Rare Earth Elements —,’” Science & Technology Trends, no. 38, pp. 40–54, 2011. [14] I. S. Moosa, “History and Development of Permanent Magnets,” vol. 2, no. 1, pp. 18–26, 2014. [15] G. Bai, R. W. Gao, Y. Sun, G. B. Han, and B. Wang, “Study of high-coercivity sintered NdFeB magnets,” J Magn Magn Mater, vol. 308, no. 1, pp. 20–23, 2007, doi: 10.1016/j.jmmm.2006.04.029. [16] X. T. Tang, Z. W. Lu, and A. Z. Sun, “The effect of sintered Nd-Fe-B with Dy infiltration to the plating crafts,” J Magn Magn Mater, vol. 475, no. November 2018, pp. 10–13, 2019, doi: 10.1016/j.jmmm.2018.11.080. [17] X. G. Cui et al., “Magnetic properties and microstructure of sintered Nd–Fe–B magnets with intergranular addition of Ni powders,” J Alloys Compd, vol. 726, pp. 846–851, 2017, doi: 10.1016/j.jallcom.2017.08.061. [18] P. Zhang, L. Liang, J. Jin, Y. Zhang, X. Liu, and M. Yan, “Magnetic properties and corrosion resistance of Nd-Fe-B magnets with Nd64Co36intergranular addition,” J Alloys Compd, vol. 616, pp. 345–349, 2014, doi: 10.1016/j.jallcom.2014.07.085. [19] C. Jin et al., “Magnetic properties and phase evolution of sintered Nd-Fe-B magnets with intergranular addition of Pr–Co alloy,” J Alloys Compd, vol. 670, pp. 72–77, 2016, doi: 10.1016/j.jallcom.2016.02.006. [20] P. Zhang, T. Ma, L. Liang, and M. Yan, “Influence of Ta intergranular addition on microstructure and corrosion resistance of Nd-Dy-Fe-B sintered magnets,” J Alloys Compd, vol. 593, pp. 137–140, 2014, doi: 10.1016/j.jallcom.2014.01.055. [21] L. Li et al., “A novel method combining additive manufacturing and alloy infiltration for NdFeB bonded magnet fabrication,” J Magn Magn Mater, vol. 438, pp. 163–167, 2017, doi: 10.1016/j.jmmm.2017.04.066. [22] T. Sato, N. Oka, T. Ohsuna, Y. Kaneko, S. Suzuki, and T. Shima, “Enhancement of coercivity for Nd-Fe-B thin films by the infiltration of Nd-Cu alloy cap layer,” J Appl Phys, vol. 110, no. 2, pp. 1–5, 2011, doi: 10.1063/1.3608244. [23] W. Francis, “Definitions and Units,” Fuels and Fuel Technology, pp. 3–8, 2013, doi: 10.1016/b978-0-08-025250-6.50006-7. [24] T. Magnetic, “1 . 1 . 2 BASIC OPERATING PRINCIPLE OF ELECTRIC MOTORS,” no. 2017, pp. 56–58, 2023. [25] A. Hughes, Electric motors and drives [electronic resource] : fundamentals, types and applications, 3rd ed. Amsterdam ; Boston ; London: Elsevier Newnes, 2006. [26] A. E. Fitzgerald and S. D. Umans, Electric machinery, 6th ed. Boston, Mass. ; London: McGraw-Hill, 2003. [27] T. J. E. Miller, Brushless permanent-magnet and reluctance motor drives, 2nd (Corr.)impression. Oxford: Clarendon, 1993. [28] M. Šustek, M. Marcaník, P. Tomášek, and Z. Úředníček, “DC motors and servo-motors controlled by Raspberry Pi 2B,” MATEC Web of Conferences, vol. 125, pp. 1–6, 2017, doi: 10.1051/matecconf/201712502025. [29] J. R. Hendershot and T. J. E. Miller, Design of brushless permanent-magnet motors. Hillsboro, OH : Oxford: Magna Pysics Pub. ; Clarendon Press, 1994. [30] B. K. Bose, Modern power electronics and AC drives. Upper Saddle River, NJ: Prentice Hall PTR, 2002. [31] C. J. Fraser, “Electrical machines,” The Mechatronics Handbook, pp. 20-33-20–51, 2002, doi: 10.1201/9781420037043-13. [32] U. of LaSalle, “Magnetic Susceptibility,” Notes, no. May, pp. 4–7, 2014. [33] J. M. D. Coey, “Ferromagnetism and exchange,” in Magnetism and Magnetic Materials, 2010, pp. 128–129. doi: https://doi.org/10.1017/CBO9780511845000.006. [34] J. M. D. Coey, “Antiferromagnetism and other magnetic order,” in Magnetism and Magnetic Materials, 2010, pp. 195–230. doi: https://doi.org/10.1017/CBO9780511845000.007. [35] O. Fabiyi, “Chapter 3. Methodology,” Gated Neighbourhoods and privatisation of urban security in Ibadan Metropolis, pp. 27–29, 2016, doi: 10.4000/books.ifra.475. [36] E. P. Wohlfarth, “Hard magnetic materials,” Adv Phys, vol. 8, no. 30, pp. 87–224, 1959, doi: 10.1080/00018735900101178. [37] “6.9: Hard and Soft Magnets - Chemistry LibreTexts,” vol. 310, p. 189204, [Online]. Available: https://chem.libretexts.org/Bookshelves/Inorganic_Chemistry/Book%3A_Introduction_to_Inorganic_Chemistry/06%3A_Metals_and_Alloys-_Structure_Bonding_Electronic_and_Magnetic_Properties/6.09%3A_Hard_and_Soft_Magnets [38] H. R.Kirchmayr, “REVIEW ARTICLE Permanent magnets and hard magnetic materials,” J Appl Phys, vol. 29, pp. 2763–2778, 1996. [39] J. Karlsson and O. Söderström, “Review of Magnetic Materials Along With a Study of the Magnetic Stability and Solidity of Y40,” no. June, 2012, [Online]. Available: https://www.diva-portal.org/smash/get/diva2:534040/FULLTEXT01.pdf [40] L. H. Lewis and F. Jiménez-Villacorta, “Perspectives on permanent magnetic materials for energy conversion and power generation,” Metall Mater Trans A Phys Metall Mater Sci, vol. 44, no. SUPPL. 1, 2013, doi: 10.1007/s11661-012-1278-2. [41] eclipsemagnetics, “Magnet Materials & Assemblies - Sector Expertise - Power Generation.” https://www.eclipsemagnetics.com/row/magnet-materials-and-assemblies/?gclid=EAIaIQobChMI3q3V8ami4QIVGLLtCh2Klw_LEAAYASAAEgI_1_D_BwE [42] Sas.usace.army.mil., “Savannah District > About > Divisions and Offices > Operations Division > Richard B. Russell Dam and Lake > Hydropower > How Hydropower Works.” https://www.sas.usace.army.mil/About/Divisions-and-Offices/Operations-Division/Richard-B-Russell-Dam-and-Lake/Hydropower/ [43] H. Shokrollahi and K. Janghorban, “Soft magnetic composite materials (SMCs),” J Mater Process Technol, vol. 189, no. 1–3, pp. 1–12, 2007, doi: 10.1016/j.jmatprotec.2007.02.034. [44] J. E. Lenz, “A review of magnetic sensors,” Proceedings of the IEEE, vol. 78, no. 6, pp. 973–989, 1990. [45] McLaren Applied Technologies, “Permanent Magnet Alternator.” https://www.mclaren.com/appliedtechnologies/products/item/alternator-permanent-magnet/ [46] Adams Magnetic Products, “Magnets for Motor Applications.” https://www.adamsmagnetic.com/markets/magnets-motor-applications [47] Goudsmit, “Permanent Magnets and Precision Machined Parts for Medical Devices.” https://www.goudsmit.co.uk/sectors/medical/ [48] Q. A. Pankhurst, J. Connolly, S. K. Jones, and J. Dobson, “1110.J.Phys.D Appl.Phys.2003,36,R167.pdf,” vol. 36, 2003, doi: 10.1088/0022-3727/36/13/201. [49] M. A. Riley, A. D. Walmsley, J. D. Speight, and I. R. Harris, “Magnets in medicine,” Materials Science and Technology, vol. 18, no. 1, pp. 1–12, 2003, doi: 10.1179/026708301125000140. [50] A. du Plessis et al., “Standard method for microCT-based additive manufacturing quality control 2: Density measurement,” MethodsX, vol. 5, no. September, pp. 1117–1123, 2018, doi: 10.1016/j.mex.2018.09.006. [51] C. Rong and B. Shen, “Nanocrystalline and nanocomposite permanent magnets by melt spinning technique,” Chinese Physics B, vol. 27, no. 11, p. 117502, 2018, doi: 10.1088/1674-1056/27/11/117502. [52] B. J. F. Herbst, J. J. Croat, and F. E. Pinkerton, “Relationships Between Crystal Structure and Magnetic Properties in Nd 2 Fe 14 B,” no. April, 1984, doi: 10.1103/PhysRevB.29.4176. [53] K. Hono, “Strategy for high-coercivity Nd – Fe – B magnets,” Scr Mater, vol. 67, no. 6, pp. 530–535, 2012, doi: 10.1016/j.scriptamat.2012.06.038. [54] N. Magnets, “Mikrochimica Acta Metallurgical Factors Determining the Coercivity of,” pp. 115–124, 1987. [55] T. Shujian, L. Qingfan, L. Shixiang, and Z. Chaogui, “Phase diagram of the ternary system CeCl3-KCl-LiCl,” J Alloys Compd, vol. 274, no. 1–2, pp. 142–147, 1998, doi: 10.1016/S0925-8388(98)00551-9. [56] C. V. Mikler, V. Chaudhary, V. Soni, B. Gwalani, R. V. Ramanujan, and R. Banerjee, “Tuning the phase stability and magnetic properties of laser additively processed Fe-30at%Ni soft magnetic alloys,” Mater Lett, vol. 199, pp. 88–92, 2017, doi: 10.1016/j.matlet.2017.04.054. [57] X. Chen et al., “Laser additive processing of Fe-Si-B-Cu-Nb magnetic alloys,” J Manuf Process, vol. 29, pp. 175–181, 2017, doi: 10.1016/j.jmapro.2017.07.029. [58] C. V. Mikler et al., “Laser Additive Manufacturing of Magnetic Materials,” Jom, vol. 69, no. 3, pp. 532–543, 2017, doi: 10.1007/s11837-017-2257-2. [59] C. V. Mikler et al., “Laser additive processing of Ni-Fe-V and Ni-Fe-Mo Permalloys: Microstructure and magnetic properties,” Mater Lett, vol. 192, pp. 9–11, 2017, doi: 10.1016/j.matlet.2017.01.059. [60] B. Heer and A. Bandyopadhyay, “Compositionally graded magnetic-nonmagnetic bimetallic structure using laser engineered net shaping,” Mater Lett, vol. 216, pp. 16–19, 2018, doi: 10.1016/j.matlet.2017.12.129. [61] E. M. H. White, A. G. Kassen, E. Simsek, W. Tang, R. T. Ott, and I. E. Anderson, “Net Shape Processing of Alnico Magnets by Additive Manufacturing,” IEEE Trans Magn, vol. 53, no. 11, 2017, doi: 10.1109/TMAG.2017.2711965. [62] L. M. Bollig, P. J. Hilpisch, G. S. Mowry, and B. B. Nelson-Cheeseman, “3D printed magnetic polymer composite transformers,” J Magn Magn Mater, vol. 442, pp. 97–101, 2017, doi: 10.1016/j.jmmm.2017.06.070. [63] C. Huber et al., “3D print of polymer bonded rare-earth magnets, and 3D magnetic field scanning with an end-user 3D printer,” Appl Phys Lett, vol. 109, no. 16, 2016, doi: 10.1063/1.4964856. [64] S. J. Leigh, C. P. Purssell, D. R. Billson, and D. A. Hutchins, “Using a magnetite/thermoplastic composite in 3D printing of direct replacements for commercially available flow sensors,” Smart Mater Struct, vol. 23, no. 9, 2014, doi: 10.1088/0964-1726/23/9/095039. [65] L. Lu, P. Guo, and Y. Pan, “Magnetic-Field-Assisted Projection Stereolithography for Three-Dimensional Printing of Smart Structures,” J Manuf Sci Eng, vol. 139, no. 7, p. 071008, 2017, doi: 10.1115/1.4035964. [66] V. Popov, A. Koptyug, I. Radulov, F. Maccari, and G. Muller, “Prospects of additive manufacturing of rare-earth and non-rare-earth permanent magnets,” Procedia Manuf, vol. 21, no. 2017, pp. 100–108, 2018, doi: 10.1016/j.promfg.2018.02.199. [67] L. Li et al., “Big Area Additive Manufacturing of High Performance Bonded NdFeB Magnets,” Sci Rep, vol. 6, no. October, pp. 1–7, 2016, doi: 10.1038/srep36212. [68] L. Li, B. Post, V. Kunc, A. M. Elliott, and M. P. Paranthaman, “Additive manufacturing of near-net-shape bonded magnets: Prospects and challenges,” Scr Mater, vol. 135, pp. 100–104, 2017, doi: 10.1016/j.scriptamat.2016.12.035. [69] M. P. Paranthaman et al., “Binder Jetting : A Novel NdFeB Bonded Magnet Fabrication Process,” vol. 68, no. 7, pp. 1978–1982, 2016, doi: 10.1007/s11837-016-1883-4. [70] C. Vyas, G. Poologasundarampillai, J. Hoyland, and P. Bartolo, “12 - 3D printing of biocomposites for osteochondral tissue engineering,” in Biomedical Composites, 2017, pp. 261–302. doi: https://doi.org/10.1016/B978-0-08-100752-5.00013-5. [71] K. Anderson, C. Skelly, K. L. Martinson, K. L. Waite, P. M. Auwerda, and G. Heyboer, “Simultaneous multi-state equine business education program,” J Equine Vet Sci, vol. 33, no. 5, p. 389, 2013, doi: 10.1016/j.jevs.2013.03.154. [72] D. Herzog, V. Seyda, E. Wycisk, and C. Emmelmann, “Additive manufacturing of metals,” Acta Mater, vol. 117, pp. 371–392, 2016, doi: 10.1016/j.actamat.2016.07.019. [73] B. Zhang, N. E. Fenineche, L. Zhu, H. Liao, and C. Coddet, “Studies of magnetic properties of permalloy (Fe30%Ni) prepared by SLM technology,” J Magn Magn Mater, vol. 324, no. 4, pp. 495–500, 2012, doi: 10.1016/j.jmmm.2011.08.030. [74] B. Zhang, N. E. Fenineche, H. Liao, and C. Coddet, “Microstructure and magnetic properties of Fe-Ni alloy fabricated by selective laser melting Fe/Ni mixed powders,” J Mater Sci Technol, vol. 29, no. 8, pp. 757–760, 2013, doi: 10.1016/j.jmst.2013.05.001. [75] B. Zhang, N. E. Fenineche, H. Liao, and C. Coddet, “Magnetic properties of in-situ synthesized FeNi3 by selective laser melting Fe-80%Ni powders,” J Magn Magn Mater, vol. 336, pp. 49–54, 2013, doi: 10.1016/j.jmmm.2013.02.014. [76] T. Bauer, A. B. Spierings, and K. Wegener, “Microstructure and Electro-Magnetic Properties of a Nickel-Based Anti-Magnetic Shielding Alloy,” Proceedings of the 27th Annual International Solid Freeform Fabrication Symposium 2016, pp. 1856–1867, 2016. [77] K. J. Jhong, W. C. Huang, and W. H. Lee, “Microstructure and magnetic properties of magnetic material fabricated by selective laser melting,” Phys Procedia, vol. 83, pp. 818–824, 2016, doi: 10.1016/j.phpro.2016.08.084. [78] T. Kolb et al., “Laser Beam Melting of NdFeB for the production of rare-earth magnets,” 2016 6th International Electric Drives Production Conference, EDPC 2016 - Proceedings, pp. 34–40, 2016, doi: 10.1109/EDPC.2016.7851311. [79] N. Urban, F. Huber, and J. Franke, “Influences of process parameters on rare earth magnets produced by laser beam melting,” 2017 7th International Electric Drives Production Conference, EDPC 2017 - Proceedings, vol. 2017-Decem, pp. 1–5, 2018, doi: 10.1109/EDPC.2017.8328149. [80] D. Goll et al., “Refining the Microstructure of Fe-Nd-B by Selective Laser Melting,” Physica Status Solidi - Rapid Research Letters, vol. 13, no. 3, pp. 1–5, 2019, doi: 10.1002/pssr.201800536. [81] M. Skalon et al., “Influence of Melt-Pool Stability in 3D Printing of NdFeB Magnets on Density and Magnetic Properties,” Materials, vol. 13, no. 1, p. 139, 2019, doi: 10.3390/ma13010139. [82] D. Goll, F. Trauter, T. Bernthaler, J. Schanz, H. Riegel, and G. Schneider, “Additive manufacturing of bulk nanocrystalline fendb based permanent magnets,” Micromachines (Basel), vol. 12, no. 5, 2021, doi: 10.3390/mi12050538. [83] J. Wu, N. T. Aboulkhair, M. Degano, I. Ashcroft, and R. J. M. Hague, “Process-structure-property relationships in laser powder bed fusion of permanent magnetic Nd-Fe-B,” Mater Des, vol. 209, p. 109992, 2021, doi: 10.1016/j.matdes.2021.109992. [84] N. Urban, A. Meyer, S. Kreitlein, F. Leicht, and J. Franke, “Efficient near Net-Shape Production of High Energy Rare Earth Magnets by Laser Beam Melting,” Applied Mechanics and Materials, vol. 871, pp. 137–144, 2017, doi: 10.4028/www.scientific.net/amm.871.137. [85] F. Bittner, J. Thielsch, and W. G. Drossel, “Laser powder bed fusion of Nd–Fe–B permanent magnets,” Progress in Additive Manufacturing, vol. 5, no. 1, pp. 3–9, 2020, doi: 10.1007/s40964-020-00117-7. [86] F. Vial, F. Joly, E. Nevalainen, M. Sagawa, K. Hiraga, and K. T. Park, “Improvement of coercivity of sintered NdFeB permanent magnets by heat treatment,” J Magn Magn Mater, vol. 242–245, pp. 1329–1334, 2002, doi: 10.1016/S0304-8853(01)00967-2. [87] Y. Zhang et al., “Post-sinter annealing influences on coercivity of multi-main-phase Nd-Ce-Fe-B magnets,” Acta Mater, vol. 146, pp. 97–105, 2018, doi: 10.1016/j.actamat.2017.12.027. [88] N. Emminghaus, C. Hoff, J. Hermsdorf, and S. Kaierle, “Laser Powder Bed Fusion of NdFeB and influence of heat treatment on microstructure and crack development,” Procedia CIRP, vol. 94, pp. 211–216, 2020, doi: 10.1016/j.procir.2020.09.040. [89] H. R. Cha, K. W. Jeon, J. H. Yu, H. W. Kwon, Y. Do Kim, and J. G. Lee, “Coercivity enhancement of hot-deformed Nd-Fe-B magnet by grain boundary diffusion process using the reaction of NdHxand Cu nanopowders,” J Alloys Compd, vol. 693, pp. 744–748, 2017, doi: 10.1016/j.jallcom.2016.09.167. [90] M. Tang et al., “Microstructure modification and coercivity enhancement of Nd-Ce-Fe-B sintered magnets by grain boundary diffusing Nd-Dy-Al alloy,” J Magn Magn Mater, vol. 442, pp. 338–342, 2017, doi: 10.1016/j.jmmm.2017.06.116. [91] S. Guo, X. Zhang, G. Ding, R. Chen, D. Lee, and A. Yan, “Coercivity enhancement of sintered Nd-Fe-B magnets by chemical bath deposition of TbCl3,” J Appl Phys, vol. 115, no. 17, pp. 23–26, 2014, doi: 10.1063/1.4867962. [92] W. F. Li, T. Ohkubo, K. Hono, and M. Sagawa, “The origin of coercivity decrease in fine grained Nd-Fe-B sintered magnets,” J Magn Magn Mater, vol. 321, no. 8, pp. 1100–1105, 2009, doi: 10.1016/j.jmmm.2008.10.032. [93] H. W. Chang, Y. I. Lee, P. H. Liao, and W. C. Chang, “Significant coercivity enhancement of hot deformed NdFeB magnets by doping Ce-containing (PrNdCe)70Cu30 alloys powders,” Scr Mater, vol. 146, pp. 222–225, 2018, doi: 10.1016/j.scriptamat.2017.11.052. [94] X. Zheng et al., “Coercivity enhancement by inhibiting the formation of coarse grains region in hot-deformed Nd-Fe-B magnets with WC nano-particles addition,” Scr Mater, vol. 132, pp. 49–52, 2017, doi: 10.1016/j.scriptamat.2017.01.024. [95] X. Zhang et al., “Improvement of the thermal stability of sintered Nd-Fe-B magnets by intergranular addition of Dy82.3Co17.7,” J Appl Phys, vol. 115, no. 17, pp. 3–6, 2014, doi: 10.1063/1.4868491. [96] F. Bittner, J. Thielsch, and W. G. Drossel, “Microstructure and magnetic properties of Nd-Fe-B permanent magnets produced by laser powder bed fusion,” Scr Mater, vol. 201, p. 113921, 2021, doi: 10.1016/j.scriptamat.2021.113921. [97] S. Godavarthi, J. Porcayo-Calderon, E. Vazquez-Velez, M. Casales-Diaz, D. M. Ortega-Toledo, and L. Martinez-Gomez, “Influence of the chemical composition in the electrochemical response of permanent magnets,” Journal of Spectroscopy, vol. 2015, 2015, doi: 10.1155/2015/356027. [98] X. Y. Fang, D. Q. Yi, J. F. Nie, X. J. Zhang, B. Wang, and L. R. Xiao, “Effect of Zr, Mn and Sc additions on the grain size of Mg-Gd alloy,” J Alloys Compd, vol. 470, no. 1–2, pp. 311–316, 2009, doi: 10.1016/j.jallcom.2008.02.069. [99] H. W. Chang, C. H. Chiu, C. W. Chang, W. C. Chang, A. C. Sun, and Y. D. Yao, “Effect of Ti substitution on the magnetic properties, microstructure, and aftereffect of melt spun PrFeB nanocomposites,” Scr Mater, vol. 55, no. 6, pp. 529–532, 2006, doi: 10.1016/j.scriptamat.2006.05.032. [100] T. H. Coil, “Helmholtz coils Helmholtz coils,” no. 5. [101] LakeShore, “Measuring Permanent Magnet Characteristics with a Fluxmeter and Helmholtz Coil,” no. 614, 2010, [Online]. Available: www.lakeshore.com [102] T. Eb, “Chapter 4 Magnetic properties of the layer systems measured by SQUID magnetometry,” Measurement, pp. 27–40. [103] H. Gong, K. Rafi, H. Gu, T. Starr, and B. Stucker, “Analysis of defect generation in Ti-6Al-4V parts made using powder bed fusion additive manufacturing processes,” Addit Manuf, vol. 1, pp. 87–98, 2014, doi: 10.1016/j.addma.2014.08.002. [104] C. Chen, S. Chang, J. Zhu, Z. Xiao, H. Zhu, and X. Zeng, “Residual stress of typical parts in laser powder bed fusion,” J Manuf Process, vol. 59, no. October, pp. 621–628, 2020, doi: 10.1016/j.jmapro.2020.10.009. [105] E. Toyserkani et al., “Experimental and numerical investigation on the effect of layer thickness during laser powder-bed fusion of stainless steel 17-4PH,” International Journal of Rapid Manufacturing, vol. 9, no. 2/3, p. 1, 2020, doi: 10.1504/ijrapidm.2020.10029113. [106] X. Shi, C. Yan, W. Feng, Y. Zhang, and Z. Leng, “Effect of high layer thickness on surface quality and defect behavior of Ti-6Al-4V fabricated by selective laser melting,” Opt Laser Technol, vol. 132, no. June, p. 106471, 2020, doi: 10.1016/j.optlastec.2020.106471. [107] “White-paper1-EN”. [108] N. T. Oster, “Generation and characterization of anisotropic microstructures in rare earth-iron-boron alloys,” p. 134, 2012. [109] N. Sridharan et al., “Rationalization of solidification mechanism of Nd–Fe–B magnets during laser directed-energy deposition,” J Mater Sci, vol. 53, no. 11, pp. 8619–8626, 2018, doi: 10.1007/s10853-018-2178-7. [110] R. Li, Y. Shi, Z. Wang, L. Wang, J. Liu, and W. Jiang, “Densification behavior of gas and water atomized 316L stainless steel powder during selective laser melting,” Appl Surf Sci, vol. 256, no. 13, pp. 4350–4356, 2010, doi: 10.1016/j.apsusc.2010.02.030. [111] S. Waqar, K. Guo, and J. Sun, “Evolution of residual stress behavior in selective laser melting (SLM) of 316L stainless steel through preheating and in-situ re-scanning techniques,” Opt Laser Technol, vol. 149, no. June 2021, p. 107806, 2022, doi: 10.1016/j.optlastec.2021.107806. [112] M. M. Savalani and J. M. Pizarro, “Effect of preheat and layer thickness on selective laser melting (SLM) of magnesium,” Rapid Prototyp J, vol. 22, no. 1, pp. 115–122, 2016, doi: 10.1108/RPJ-07-2013-0076. [113] A. Mazilkin et al., “Grain boundary oxide layers in NdFeB-based permanent magnets,” Mater Des, vol. 199, p. 109417, 2021, doi: 10.1016/j.matdes.2020.109417. [114] T. de Terris et al., “Optimization and comparison of porosity rate measurement methods of Selective Laser Melted metallic parts,” Addit Manuf, vol. 28, no. May, pp. 802–813, 2019, doi: 10.1016/j.addma.2019.05.035. [115] M. Heydarzadeh Sohi, M. Ebrahimi, A. Honarbakhsh Raouf, and F. Mahboubi, “Comparative study of the corrosion behaviour of plasma nitrocarburised AISI4140 steel before and after post-oxidation,” Mater Des, vol. 31, no. 9, pp. 4432–4437, 2010, doi: 10.1016/j.matdes.2010.04.017. [116] C. Huber et al., “Coercivity enhancement of selective laser sintered NdFeB magnets by grain boundary infiltration,” Acta Mater, vol. 172, pp. 66–71, 2019, doi: 10.1016/j.actamat.2019.04.037. [117] A. S. Volegov et al., “Additive manufacturing of heavy rare earth free high-coercivity permanent magnets,” Acta Mater, vol. 188, pp. 733–739, 2020, doi: 10.1016/j.actamat.2020.02.058. [118] K. Essa, P. Jamshidi, J. Zou, M. M. Attallah, and H. Hassanin, “Porosity control in 316L stainless steel using cold and hot isostatic pressing,” Mater Des, vol. 138, pp. 21–29, 2018, doi: 10.1016/j.matdes.2017.10.025. [119] H. V. Atkinson and S. Davies, “Fundamental aspects of hot isostatic pressing: An overview,” Metall Mater Trans A Phys Metall Mater Sci, vol. 31, no. 12, pp. 2981–3000, 2000, doi: 10.1007/s11661-000-0078-2. [120] F. Yang et al., “Performance of Nd-Fe-B Magnets Fabricated by Hot Isostatic Pressing and Low-Temperature Sintering,” J Mater Eng Perform, vol. 28, no. 1, pp. 273–277, 2019, doi: 10.1007/s11665-018-3832-6. [121] Z. Q. Liao, F. Xu, W. J. Yan, Q. J. Huang, G. Chen, and S. D. Li, “Influence of cladless hot isostatic pressing on magnetic properties and corrosion resistance of sintered NdFeB magnets,” Key Eng Mater, vol. 538, pp. 211–214, 2013, doi: 10.4028/www.scientific.net/KEM.538.211. [122] J. Liu et al., “Grain size dependence of coercivity of hot-deformed Nd-Fe-B anisotropic magnets,” Acta Mater, vol. 82, pp. 336–343, 2015, doi: 10.1016/j.actamat.2014.09.021."],"dcterms:accessrights":["public"],"dc:title":["Processing of NdFeB for Electric Motor Applications Using Selective Laser Melting"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"]},"updated_at":"2026-11-18T23:22:02Z"}