{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:35352"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:35352","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Scaling Up The Tribological Assessment of Laser Clad Rail to Build The Case For Field Implementation","abstract":"The wheel/rail contact in railways is one of the most examined parts and from the beginning of railway travel new solutions were needed to optimise its performance. Wear and rolling contact fatigue (RCF) are the two biggest problems. Those problems directly affect the rail and wheel life in the railway industry. When rails have high deformation (taking the rail profile outside of acceptable geometrical thresholds defined by standards) or damage, they need to be taken out and replaced and that causes many delays and problems. This would be longer in lighter traffic lines, but in heavy and mostly used traffic lines the rail life is 2-3 years. Surface treatment methods increase the lifetime of rails and coating over rail surface have given good solution for those problems. Laser cladding is an additive manufacturing coating method. It allows the same or a different type of material to be coated over a rail or wheel substrate. Laser cladding process parameters and material selections are important factors for achieving this purpose. In this thesis work showed that laser clad coated rail specimens tested under different test scales: small-scale tests, full-scale tests in laboratory conditions and field tests with actual environmental conditions. Material selection of laser clad specimens was based on previous tests for improved wear and RCF resistance. They were compared with standard grade rails and premium rails. The clad materials were martensitic stainless steel (MSS), Stellite 6, R260, and T400. The substrate rail material used was R260 grade rail. Also, some premium rail tests were conducted for comparison: Manganese (Mn), Chromium (Cr) and R400 HT. Small-scale twin disc tests were conducted to find the full lifespan of MSS clad and some repair solutions with MSS clad, Stellite 6 clad and R260 clad over R260 rail specimen “damage”. The premium rail specimens were analysed and compared with R260 rail specimen and MSS clad specimens. Also, laser cladding process parameters were changed with MSS clad over R260 rail and tested to find how clad “quality” affects the performance of clad specimens and how defects change or cause problems when optimal clad parameters changed. Full-scale tests were conducted to see how clad specimens and repair specimens perform under actual loading conditions. MSS clad, Stellite 6 clad and R260 un-clad pocket specimens were analysed and compared with small scale tests. A T400 rail specimen was tested for repair analysis. The results of small-scale tests were reflected in the full-scale test outcomes. In all tests the clad layers performed well in terms of wear and RCF resistance which gave the confidence needed to initiate field tests. MSS clad twin-disc experiments showed that the clad disc did not fail over 400,000 cycles. However, experiments with R260 standard grade rail discs observed failures occurring around 15,000 cycles in the literature. It is evident that the MSS clad disc exhibited at least 20-25 times higher wear and rolling contact fatigue (RCF) resistance than the standard grade rail disc. These were started, and data collection undertaken for R260 rails, HP 335 premium rails, MSS clad rails with different clad thickness, Stellite 6 clad rails, and insulated block joint (IBJ) components.","abstract_html":"The wheel/rail contact in railways is one of the most examined parts and from the beginning of railway travel new solutions were needed to optimise its performance. Wear and rolling contact fatigue (RCF) are the two biggest problems. Those problems directly affect the rail and wheel life in the railway industry. When rails have high deformation (taking the rail profile outside of acceptable geometrical thresholds defined by standards) or damage, they need to be taken out and replaced and that causes many delays and problems. This would be longer in lighter traffic lines, but in heavy and mostly used traffic lines the rail life is 2-3 years. Surface treatment methods increase the lifetime of rails and coating over rail surface have given good solution for those problems. Laser cladding is an additive manufacturing coating method. It allows the same or a different type of material to be coated over a rail or wheel substrate. Laser cladding process parameters and material selections are important factors for achieving this purpose. In this thesis work showed that laser clad coated rail specimens tested under different test scales: small-scale tests, full-scale tests in laboratory conditions and field tests with actual environmental conditions. Material selection of laser clad specimens was based on previous tests for improved wear and RCF resistance. They were compared with standard grade rails and premium rails. The clad materials were martensitic stainless steel (MSS), Stellite 6, R260, and T400. The substrate rail material used was R260 grade rail. Also, some premium rail tests were conducted for comparison: Manganese (Mn), Chromium (Cr) and R400 HT. Small-scale twin disc tests were conducted to find the full lifespan of MSS clad and some repair solutions with MSS clad, Stellite 6 clad and R260 clad over R260 rail specimen “damage”. The premium rail specimens were analysed and compared with R260 rail specimen and MSS clad specimens. Also, laser cladding process parameters were changed with MSS clad over R260 rail and tested to find how clad “quality” affects the performance of clad specimens and how defects change or cause problems when optimal clad parameters changed. Full-scale tests were conducted to see how clad specimens and repair specimens perform under actual loading conditions. MSS clad, Stellite 6 clad and R260 un-clad pocket specimens were analysed and compared with small scale tests. A T400 rail specimen was tested for repair analysis. The results of small-scale tests were reflected in the full-scale test outcomes. In all tests the clad layers performed well in terms of wear and RCF resistance which gave the confidence needed to initiate field tests. MSS clad twin-disc experiments showed that the clad disc did not fail over 400,000 cycles. However, experiments with R260 standard grade rail discs observed failures occurring around 15,000 cycles in the literature. It is evident that the MSS clad disc exhibited at least 20-25 times higher wear and rolling contact fatigue (RCF) resistance than the standard grade rail disc. These were started, and data collection undertaken for R260 rails, HP 335 premium rails, MSS clad rails with different clad thickness, Stellite 6 clad rails, and insulated block joint (IBJ) components.","abstract_has_math":false,"creators":["YILDIRIMLI, KAZIM"],"institution":"University of Sheffield","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Lewis, Roger","Fletcher, David"],"committee_chairs":[],"committee_members":[],"year":2024,"date_issued":"2024-07","date_published":"2024-07","updated_at":"2026-11-18T23:27:24Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[],"person_identifier_entries":[{"key":"person:identifier.orcid","label":"ORCID","values":["0000000177398342"],"render_values":[{"text":"0000-0001-7739-8342","href":"https://orcid.org/0000-0001-7739-8342","code":true}]}]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/35352/1/Kazim%20Yildirimli_Scaling%20Up%20The%20Tribological%20Assessment%20of%20Laser%20Clad%20Rail%20to%20Build%20The%20Case%20For%20Field%20Implementation.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A35352","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Lewis, Roger","Fletcher, David"]},{"key":"dc:creator","label":"Author","values":["YILDIRIMLI, KAZIM"]},{"key":"person:identifier.orcid","label":"ORCID","values":["0000000177398342"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2024-07"]},{"key":"dc:date.issued","label":"Date","values":["2024-07"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Mechanical Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/35352/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["AbrasiMet 250. (n.d.).“AbrasiMet 250B Brochure.” [Online]. Available at: https://www.buehler.com/assets/Brochures/English/Sectioning/AbrasiMet250Brochure.pdf. Athukorala, A., & De Pellegrin, D. V. (2017). Experimental Depiction of the Hypothesis of Flake-Like Wear Debris Generation in Rolling Contact Fatigue of the Rail–Wheel Contact Interface. Tribology Transactions, 60(4), 581–591. https://doi.org/10.1080/10402004.2016.1188189 Ayrault, S., Chateauminois, A., Soulier, J. P., Tréheux, D., & Vannes, A. B. (1996). Deposition of a ceramic coating on a thermoplastic polymer by atmospheric plasma and laser cladding. Surface and Coatings Technology. https://doi.org/10.1016/0257-8972(95)02432-8 Beaty, P., Temple, B., Marshall, M. B., & Lewis, R. (2015). Experimental modelling of lipping in insulated rail joints and investigation of rail head material improvements. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 230(4), 1375–1387. https://doi.org/10.1177/0954409715600740 Bhadeshia, H., & Honeycombe, R. (2006). Steels: Microstructure and Properties. In Steels: Microstructure and Properties. https://doi.org/10.1016/B978-0-7506-8084-4.X5000-6 Bolton, P. J., & Clayton, P. (1984). Rolling-sliding wear damage in rail and tyre steels. Wear. https://doi.org/10.1016/0043-1648(84)90066-8 Brunskill, H. P., Zhou, L., Lewis, R., Marshall, M. B., & Dwyer-Joyce, R. S. (2012). Dynamic characterisation of the wheel/rail contact using ultrasonic reflectometry. 9th International Conference on Contact Mechanics and Wear of Rail/Wheel Systems, CM 2012, January, 98–102. https://doi.org/10.4203/ccp.104.185 Buckley-Johnstone, L., Harmon, M., Lewis, R., Hardwick, C., & Stock, R. (2019). A comparison of friction modifier performance using two laboratory test scales. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 233(2), 201–210. https://doi.org/10.1177/0954409718787045 Christoforou, P. (2020). Laser Cladding for use in Extreme Tribological Interfaces. Christoforou, P., Fletcher, D. I., & Lewis, R. (2019). Benchmarking of premium rail material wear. Wear, 436–437. https://doi.org/10.1016/j.wear.2019.202990 Christoforou, P., Lewis, S., Fletcher, D. I., Pavier, M. J., Mostafavi, M., Narayanan, A., & Lewis, R. (n.d.). Review of laser cladding tribology for high load applications Review of laser cladding tribology for high load applications. Chryssolouris, G., Zannis, S., Tsirbas, K., & Lalas, C. (n.d.). An Experimental Investigation of Laser Cladding. Chryssolouris, G., Zannis, S., Tsirbas, K., & Lalas, C. (2002). An experimental investigation of laser cladding. CIRP Annals - Manufacturing Technology. https://doi.org/10.1016/S0007-8506(07)61486-3 Clare, A., Olusola, O., Folkes, J., & Farayibi, P. (2011). Laser cladding for railway repair and preventative maintenance. 30th International Congress on Applications of Lasers and Electro-Optics, ICALEO 2011, September 2017, 240–249. https://doi.org/10.2351/1.4710578 Creaform3D. (n.d.). “HandySCAN BLACK 3D Laser Scanner.” [Online]. Available at: https://www.creaform3d.com/en/portable-3d-scanner-handyscan-3d. Cubus. (n.d.). “TestXpert testingsoftware, Cubus Testing software” [Online]. Available at: https://www.zwickroell.com/accessories/testxpert-testing-software/cubus-testing-software/ . DuraScan. (n.d.). “DuraScan micro hardness tester.” [Online]. Available at: http://f.jernindustri.dk/2fk3ntzke7ogxgha.pdf. EcoMet 250. (n.d.). “BUEHLER® EcoMet®250/300 Grinder-Polisher Family & AutoMet®250/300 Power Head.” [Online]. Available at: https://photos.labwrench.com/equipmentManuals/8248-3228.pdf. Ehsan Toyserkani, Amir Khajepour, & Stephen F. Corbin. (2004). Laser Cladding. Fasihi, P., Kendall, O., Abrahams, R., Mutton, P., Qiu, C., Schläfer, T., & Yan, W. (2022). Tribological Properties of Laser Cladded Alloys for Repair of Rail Components. Materials, 15(21), 7466. https://doi.org/10.3390/ma15217466 Fletcher, D. I., & Beynon, J. H. (2000). Development of a Machine for Closely Controlled Rolling Contact Fatigue and Wear Testing. Journal of Testing and Evaluation, 28(4), 267–275. https://doi.org/10.1520/jte12104j Franklin, F. J., Weeda, G. J., Kapoor, A., & Hiensch, E. J. M. (2005). Rolling contact fatigue and wear behaviour of the infrastar two-material rail. Wear, 258(7–8), 1048–1054. https://doi.org/10.1016/j.wear.2004.03.054 Fu, F., Zhang, Y., Chang, G., & Dai, J. (2016). Analysis on the physical mechanism of laser cladding crack and its influence factors. Optik, 127(1), 200–202. https://doi.org/10.1016/j.ijleo.2015.10.043 Fu, Z. K., Ding, H. H., Wang, W. J., Liu, Q. Y., Guo, J., & Zhu, M. H. (2015). Investigation on microstructure and wear characteristic of laser cladding Fe-based alloy on wheel/rail materials. Wear, 330–331, 592–599. https://doi.org/10.1016/j.wear.2015.02.053 Gao, J., Zhai, W., & Guo, Y. (2018). Wheel–rail dynamic interaction due to rail weld irregularity in high-speed railways. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 232(1), 249–261. https://doi.org/10.1177/0954409716664933 Garnham, J. E., & Beynon, J. H. (1991). The early detection of rolling-sliding contact fatigue cracks. In Wear (Vol. 44). Guo, H. ming, Wang, Q., Wang, W. jian, Guo, J., Liu, Q. yue, & Zhu, M. hao. (2015). Investigation on wear and damage performance of laser cladding Co-based alloy on single wheel or rail material. Wear, 328–329, 329–337. https://doi.org/10.1016/j.wear.2015.03.002 Heyder, R., & Maedler, K. (2015). The influence of wheel and rail material on the wear of the respective contact partner. CM 2015 - 10th International Conference on Contact Mechanics of Wheel / Rail Systems. Hitachi. (n.d.). “Hitachi Tabletop Microscope TM3030.” [Online]. Available at: https://www.hitachi-hightech.com/file/us/pdf/library/literature/TM3030_brochure_letter.pdf. HP335. (n.d.). “HP335 Rail for combatting rolling contact fatigue and wear .” [Online]. Available at: https://britishsteel.co.uk/media/323526/british-steel-hp335-datasheet.pdf. HP335. (2020). HP335 Rail for combatting rolling contact fatigue and wear. Hu, Y., Zhou, L., Ding, H. H., Tan, G. X., Lewis, R., Liu, Q. Y., Guo, J., & Wang, W. J. (2020). Investigation on wear and rolling contact fatigue of wheel-rail materials under various wheel/rail hardness ratio and creepage conditions. Tribology International. https://doi.org/10.1016/j.triboint.2019.106091 Hysitron. (n.d.). “Hysitron TS 77 Select Nanoindenter.” [Online]. Available at: https://www.bruker.com/en/products-and-solutions/test-and-measurement/nanomechanical-test-systems/hysitron-ts-77-select-nanoindenter.html. ImageJ. (n.d.). “Image Processing and Analysis” [Online]. Available at: https://imagej.nih.gov/ij/docs/intro.html. InfiniteFocusSL | 3D measurement system for form & finish | Alicona. (n.d.). Retrieved February 17, 2023, from https://www.alicona.com/products/infinitefocussl/ Kaierle, S., Barroi, A., Noelke, C., Hermsdorf, J., Overmeyer, L., & Haferkamp, H. (2012). Review on Laser Deposition Welding: From Micro to Macro. Physics Procedia. https://doi.org/10.1016/j.phpro.2012.10.046 Kendall, O., Abrahams, R., Paradowska, A., Reid, M., Qiu, C., Mutton, P., Schläfer, T., & Yan, W. (2023). Influence of multi-layer laser cladding depositions and rail curvature on residual stress in light rail components. Engineering Failure Analysis, 150. https://doi.org/10.1016/j.engfailanal.2023.107330 Kendall, O., Fasihi, P., Abrahams, R., Paradowska, A., Reid, M., Lai, Q., Qiu, C., Mutton, P., Soodi, M., & Yan, W. (2022). Application of a New Alloy and Post Processing Procedures for Laser Cladding Repairs on Hypereutectoid Rail Components. Materials, 15(15). https://doi.org/10.3390/ma15155447 Kendall, O., Paradowska, A., Abrahams, R., Reid, M., Qiu, C., Mutton, P., & Yan, W. (2023). Residual Stress Measurement Techniques for Metal Joints, Metallic Coatings and Components in the Railway Industry: A Review. In Materials (Vol. 16, Issue 1). MDPI. https://doi.org/10.3390/ma16010232 Lai, Q., Abrahams, R., Yan, W., Qiu, C., Mutton, P., Paradowska, A., Soodi, M., & Wu, X. (2019). Influences of depositing materials, processing parameters and heating conditions on material characteristics of laser-cladded hypereutectoid rails. Journal of Materials Processing Technology, 263, 1–20. https://doi.org/10.1016/j.jmatprotec.2018.07.035 Langford, G., & Sc, D. (2023). Microstructures. 1–5. Lewis, R., Christoforou, P., Wang, W. J., Beagles, A., Burstow, M., & Lewis, S. R. (2019). Investigation of the influence of rail hardness on the wear of rail and wheel materials under dry conditions (ICRI wear mapping project). Wear, 430–431(January), 383–392. https://doi.org/10.1016/j.wear.2019.05.030 Lewis, R., & Dwyer-Joyce, R. S. (2004). Wear mechanisms and transitions in railway wheel steels. In Part J: J. Engineering Tribology (Vol. 218). Lewis, R., & Olofsson, U. (2009). Basic tribology of the wheel-rail contact. In Wheel-Rail Interface Handbook. https://doi.org/10.1533/9781845696788.1.34 Lewis, S. R., Fretwell-Smith, S., Goodwin, P. S., Smith, L., Lewis, R., Aslam, M., Fletcher, D. I., Murray, K., & Lambert, R. (2016a). Improving rail wear and RCF performance using laser cladding. Wear, 366–367, 268–278. https://doi.org/10.1016/j.wear.2016.05.011 Lewis, S. R., Fretwell-Smith, S., Goodwin, P. S., Smith, L., Lewis, R., Aslam, M., Fletcher, D. I., Murray, K., & Lambert, R. (2016b). Improving rail wear and RCF performance using laser cladding. Wear, 366–367, 268–278. https://doi.org/10.1016/j.wear.2016.05.011 Lewis, S. R., Lewis, R., Evans, G., & Buckley-Johnstone, L. E. (2014). Assessment of railway curve lubricant performance using a twin-disc tester. Wear, 314(1–2), 205–212. https://doi.org/10.1016/j.wear.2013.11.033 Lewis, S. R., Lewis, R., & Fletcher, D. I. (2015a). Assessment of laser cladding as an option for repairing/enhancing rails. Wear, 330–331, 581–591. https://doi.org/10.1016/j.wear.2015.02.027 Lewis, S. R., Lewis, R., & Fletcher, D. I. (2015b). Assessment of laser cladding as an option for repairing/enhancing rails. Wear, 330–331, 581–591. https://doi.org/10.1016/j.wear.2015.02.027 Lewis, S. R., Lewis, R., Goodwin, P. S., Fretwell-Smith, S., Fletcher, D. I., Murray, K., & Jaiswal, J. (2017a). Full-scale testing of laser clad railway track; Case study – Testing for wear, bend fatigue and insulated block joint lipping integrity. Wear, 376–377, 1930–1937. https://doi.org/10.1016/j.wear.2017.02.023 Lewis, S. R., Lewis, R., Goodwin, P. S., Fretwell-Smith, S., Fletcher, D. I., Murray, K., & Jaiswal, J. (2017b). Full-scale testing of laser clad railway track; Case study – Testing for wear, bend fatigue and insulated block joint lipping integrity. Wear, 376–377(February), 1930–1937. https://doi.org/10.1016/j.wear.2017.02.023 Lewis, S. R., Lewis, R., Goodwin, P. S., Fretwell-Smith, S., Fletcher, D. I., Murray, K., & Jaiswal, J. (2017c). Full-scale testing of laser clad railway track; Case study – Testing for wear, bend fatigue and insulated block joint lipping integrity. Wear, 376–377(February), 1930–1937. https://doi.org/10.1016/j.wear.2017.02.023 Lu, P., Lewis, S. R., Fretwell-Smith, S., Fletcher, D. I., & Lewis, R. (2018). Laser cladding of rail; The effects of depositing material on lower rail grades. Proceedings of the 11th International Conference on Contact Mechanics and Wear of Rail/Wheel Systems, CM 2018, 610–617. https://doi.org/10.1016/j.wear.2019.203045 Magel, E., Mutton, P., Ekberg, A., & Kapoor, A. (2016). Rolling contact fatigue, wear and broken rail derailments. Wear, 366–367, 249–257. https://doi.org/10.1016/j.wear.2016.06.009 Mandal, N. K. N., & Peach, B. (2010). An Engineering Analysis of Insulated Rail Joints: A General Perspective. International Journal of Engineering Science and Technology, 2(8), 3964–3988. Mansouri, H., & Monshi, A. (2004). Microstructure and residual stress variations in weld zone of flash-butt welded railroads. Science and Technology of Welding and Joining, 9(3). https://doi.org/10.1179/136217104225012201 Markov, D. (1995). Laboratory tests for wear of rail and wheel steels. Wear. https://doi.org/10.1016/0043-1648(95)90184-1 Martensitic Stainless Steels. (n.d.). [Online]. Available at: https://bssa.org.uk/wp-content/uploads/2021/02/Martensitics_JB_2.pdf Microset (n.d.) “General purpose system for small to medium replication and moulding applications.” [Online]. Available at: https://www.microset.co.uk/products/50ml-system/index.html. Narayanan, A., Mostafavi, M., Pirling, T., Kabra, S., Lewis, R., Pavier, M. J., & Peel, M. J. (2019). Residual stress in laser cladded rail. Tribology International, 140(May), 105844. https://doi.org/10.1016/j.triboint.2019.105844 Nellian, A. S., Tan, K. E., Hoh, H. J., Pang, J. H. L., Christian, I., & Chua, S. Y. (2019, February 13). Microstructure and Wear Performance Assessment of Laser Cladded Rail Steel for Service Life Extension at Sharp-Radius Curves. 2018 International Conference on Intelligent Rail Transportation, ICIRT 2018. https://doi.org/10.1109/ICIRT.2018.8641613 Nextsense. (n.d.). “Calipri, Highly Precise Profile Measurement for Predictive Maintenance.” [Online]. Available at: https://www.nextsense-worldwide.com/en/industries/railway.html. Niederhauser, S., & Karlsson, B. (2005). Fatigue behaviour of Co-Cr laser cladded steel plates for railway applications. Wear, 258(7–8), 1156–1164. https://doi.org/10.1016/j.wear.2004.03.026 Nikon. (n.d.). “Eclipse LV150 and LV150A.” [Online]. Available at: https://www.bu.edu/photonics/files/2016/11/Nikon-LV150-Brochure.pdf. Nishikawa, L. P., & Goldenstein, H. (2019). Divorced Eutectoid on Heat-Affected Zone of Welded Pearlitic Rails. JOM, 71(2), 815–823. https://doi.org/10.1007/s11837-018-3213-5 Olofsson, U., Zhu, Y., Abbasi, S., Lewis, R., & Lewis, S. (2013). Tribology of the wheel-rail contact-aspects of wear, particle emission and adhesion. Vehicle System Dynamics, 51(7), 1091–1120. https://doi.org/10.1080/00423114.2013.800215 Pawlowski, L. (1999). Thick laser coatings: A review. Journal of Thermal Spray Technology. https://doi.org/10.1361/105996399770350502 Qian, L., Li, M., Zhou, Z., Yang, H., & Shi, X. (2005). Comparison of nano-indentation hardness to microhardness. Surface and Coatings Technology, 195(2–3), 264–271. https://doi.org/10.1016/j.surfcoat.2004.07.108 Roy, T., Paradowska, A., Abrahams, R., Law, M., Mutton, P., Soodi, M., & Yan, W. (2020). Residual stress in laser cladded heavy-haul rails investigated by neutron diffraction. Journal of Materials Processing Technology, 278. https://doi.org/10.1016/j.jmatprotec.2019.116511 Santa, J. F., Cuervo, P., Christoforou, P., Harmon, M., Beagles, A., Toro, A., & Lewis, R. (2019). Twin disc assessment of wear regime transitions and rolling contact fatigue in R400HT – E8 pairs. Wear, 432–433(January), 102916. https://doi.org/10.1016/j.wear.2019.05.031 Schmid, F., Burstow, M., & Clark, S. (2010). Best Practice in Wheel-rail Interface Management for Mixed Traffic Railways. University of Birmingham Press. https://books.google.co.uk/books?id=YM0hnwEACAAJ SciAps. (n.d.). “Handheld LIBS Analyser -SciAps Z-200+.” [Online]. Available at: https://www.qesnet.com/product/handheld-libs-analyser-sciaps-z-200/. Seo, J. W., Kim, J. –C, Kwon, S. J., & Jun, H. K. (2019). Effects of Laser Cladding for Repairing and Improving Wear of Rails. International Journal of Precision Engineering and Manufacturing, 20(7), 1207–1217. https://doi.org/10.1007/s12541-019-00115-y SF HT. (2017). “SF heat-treated range”. [Online]. Available at: https://uploads-ssl.webflow.com/5db81e2f6c50c20ceba8dc08/5f478fe902f03e69a35e1e32_British%20Steel%20Stress%20Free%20Range%20Data%20Sheet.pdf SimpliMet 1000. (n.d.). “Buehler SimpliMet 1000&3000 Automatic Mounting Press.” [Online]. Available at: http://www.sjstmat.com/uploadfile/2012/0118/20120118121742618.pdf. Singh, R., Kumar, D., Mishra, S. K., & Tiwari, S. K. (2014). Laser cladding of Stellite 6 on stainless steel to enhance solid particle erosion and cavitation resistance. Surface and Coatings Technology. https://doi.org/10.1016/j.surfcoat.2014.04.008 Srisungsitthisunti, P., Kaewprachum, B., Yang, Z., & Gao, G. (2022). Real-Time Quality Monitoring of Laser Cladding Process on Rail Steel by an Infrared Camera. Metals, 12(5). https://doi.org/10.3390/met12050825 StelliteTM, J., & KoteTM, D. (n.d.). “Stellite TM 6 Alloy”. [Online]. Available at: https://www.deloro.com/fileadmin/users/redakteur/006_Downloads/Data_Sheets/Deloro_MDS_Stellite6_rev00.pdf Suh, N. P. (1977). AN OVERVIEW OF THE DEL~INA~ON THEORY OF WEAR. In Wear (Vol. 44). Elsevier Sequoia S.A. Thompson, D. (2009). Railway Noise and Vibration. In Railway Noise and Vibration. https://doi.org/10.1016/B978-0-08-045147-3.X0023-0 Tomlinson, K., Fletcher, D., & Lewis, R. (2021). Measuring material plastic response to cyclic loading in modern rail steels from a minimal number of twin-disc tests: Https://Doi.Org/10.1177/0954409721993615. Toyserkani, E., Khajepour, A., & Corbin, S. (2017). Laser Cladding - A Versatile Proactive and Reactive Technology. New York. https://doi.org/10.2351/1.521888 Tyfour, W. R., Beynon, J. H., & Kapoor, A. (1995). The steady state wear behaviour of pearlitic rail steel under dry rolling-sliding contact conditions. Wear. https://doi.org/10.1016/0043-1648(94)06533-0 University of Southampton. (n.d.). “µ-VIS: Multidisciplinary, Multiscale, Microtomographic Volume Imaging” [Online], Available at: https://www.southampton.ac.uk/muvis/about/equipment/hutch.page. Vilar, R. (2001). Laser cladding. International Journal of Powder Metallurgy (Princeton, New Jersey), 37(2). https://doi.org/10.2351/1.521888 Vishnu, P. R. (2018). Solid-State Transformations in Weldments. In Welding, Brazing, and Soldering. https://doi.org/10.31399/asm.hb.v06.a0001341 Wang, W. J., Hu, J., Guo, J., Liu, Q. Y., & Zhu, M. H. (2014). Effect of laser cladding on wear and damage behaviors of heavy-haul wheel/rail materials. Wear, 311(1–2), 130–136. https://doi.org/10.1016/j.wear.2014.01.011 Wang, X., Lei, L., & Yu, H. (2021). A review on microstructural features and mechanical properties of wheels/rails cladded by laser cladding. Micromachines, 12(2), 1–16. https://doi.org/10.3390/mi12020152 Weng, F., Chen, C., & Yu, H. (2014). Research status of laser cladding on titanium and its alloys: A review. In Materials and Design. https://doi.org/10.1016/j.matdes.2014.01.077 Wesselmecking, S., Haupt, M., Ma, Y., Song, W., Hirt, G., & Bleck, W. (2021). Mechanism-controlled thermomechanical treatment of high manganese steels. Materials Science and Engineering A, 828, 142056. https://doi.org/10.1016/j.msea.2021.142056 Williams, J. (2005). Engineering tribology. In Engineering Tribology. https://doi.org/10.1017/CBO9780511805905 Xiaoyan Zeng, Zengyi Tao, Beidi Zhu, Erhua Zhou, & Kun Cui. (1996). Investigation of laser cladding ceramic-metal composite coatings: processing modes and mechanisms. Surface and Coatings Technology. https://doi.org/10.1016/0257-8972(95)02431-x Xie, T., Zhou, L., Ding, H., Zhu, Y., Yang, W., Xiao, Q., Wang, W., Guo, J., & Liu, Q. (2021). Investigation on the rolling contact fatigue behaviors of different laser cladding materials on the damaged rail. Journal of Tribology, 143(5), 1–13. https://doi.org/10.1115/1.4050690 Xin, L., Markine, V., & Shevtsov, I. (2018). Analysis of the effect of repair welding/grinding on the performance of railway crossings using field measurements and finite element modeling. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 232(3), 798–815. https://doi.org/10.1177/0954409717693960 Ya, W. (2015). Laser Materials Interactions During a Nalyses on Clad Formation , Thermal Cycles , Residual. Zanzarin, S. (2015). Laser Cladding with metallic powders. University of Trento, November, 133. Zhang, B., He, B., & Wang, H. (2022). Microstructural investigation and mechanical performance of laser cladding repaired bainite steel with AerMet100 steel. Surface and Coatings Technology, 440(April), 128498. https://doi.org/10.1016/j.surfcoat.2022.128498 Zhu, D., Wang, J., & Wang, Q. J. (2015). On the Stribeck Curves for Lubricated Counterformal Contacts of Rough Surfaces. Journal of Tribology, 137(2). https://doi.org/10.1115/1.4028881 Zhu, Y., Wang, W., Lewis, R., Yan, W., Lewis, S. R., & Ding, H. (2019). A review on wear between railway wheels and rails under environmental conditions. In Journal of Tribology (Vol. 141, Issue 12). American Society of Mechanical Engineers (ASME). https://doi.org/10.1115/1.4044464 Zhu, Y., Yang, Y., Mu, X., Wang, W., Yao, Z., & Yang, H. (2019). Study on wear and RCF performance of repaired damage railway wheels: Assessing laser cladding to repair local defects on wheels. Wear. https://doi.org/10.1016/j.wear.2019.04.028"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/35352/1/Kazim%20Yildirimli_Scaling%20Up%20The%20Tribological%20Assessment%20of%20Laser%20Clad%20Rail%20to%20Build%20The%20Case%20For%20Field%20Implementation.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["The wheel/rail contact in railways is one of the most examined parts and from the beginning of railway travel new solutions were needed to optimise its performance. Wear and rolling contact fatigue (RCF) are the two biggest problems. Those problems directly affect the rail and wheel life in the railway industry. When rails have high deformation (taking the rail profile outside of acceptable geometrical thresholds defined by standards) or damage, they need to be taken out and replaced and that causes many delays and problems. This would be longer in lighter traffic lines, but in heavy and mostly used traffic lines the rail life is 2-3 years. Surface treatment methods increase the lifetime of rails and coating over rail surface have given good solution for those problems. Laser cladding is an additive manufacturing coating method. It allows the same or a different type of material to be coated over a rail or wheel substrate. Laser cladding process parameters and material selections are important factors for achieving this purpose. In this thesis work showed that laser clad coated rail specimens tested under different test scales: small-scale tests, full-scale tests in laboratory conditions and field tests with actual environmental conditions. Material selection of laser clad specimens was based on previous tests for improved wear and RCF resistance. They were compared with standard grade rails and premium rails. The clad materials were martensitic stainless steel (MSS), Stellite 6, R260, and T400. The substrate rail material used was R260 grade rail. Also, some premium rail tests were conducted for comparison: Manganese (Mn), Chromium (Cr) and R400 HT. Small-scale twin disc tests were conducted to find the full lifespan of MSS clad and some repair solutions with MSS clad, Stellite 6 clad and R260 clad over R260 rail specimen “damage”. The premium rail specimens were analysed and compared with R260 rail specimen and MSS clad specimens. Also, laser cladding process parameters were changed with MSS clad over R260 rail and tested to find how clad “quality” affects the performance of clad specimens and how defects change or cause problems when optimal clad parameters changed. Full-scale tests were conducted to see how clad specimens and repair specimens perform under actual loading conditions. MSS clad, Stellite 6 clad and R260 un-clad pocket specimens were analysed and compared with small scale tests. A T400 rail specimen was tested for repair analysis. The results of small-scale tests were reflected in the full-scale test outcomes. In all tests the clad layers performed well in terms of wear and RCF resistance which gave the confidence needed to initiate field tests. MSS clad twin-disc experiments showed that the clad disc did not fail over 400,000 cycles. However, experiments with R260 standard grade rail discs observed failures occurring around 15,000 cycles in the literature. It is evident that the MSS clad disc exhibited at least 20-25 times higher wear and rolling contact fatigue (RCF) resistance than the standard grade rail disc. These were started, and data collection undertaken for R260 rails, HP 335 premium rails, MSS clad rails with different clad thickness, Stellite 6 clad rails, and insulated block joint (IBJ) components."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Scaling Up The Tribological Assessment of Laser Clad Rail to Build The Case For Field Implementation"]}]}],"canonical_facts":{"dc:contributor.advisor":["Lewis, Roger","Fletcher, David"],"dc:creator":["YILDIRIMLI, KAZIM"],"dc:date":["2024-07"],"dc:date.issued":["2024-07"],"dc:description.abstract":["The wheel/rail contact in railways is one of the most examined parts and from the beginning of railway travel new solutions were needed to optimise its performance. Wear and rolling contact fatigue (RCF) are the two biggest problems. Those problems directly affect the rail and wheel life in the railway industry. When rails have high deformation (taking the rail profile outside of acceptable geometrical thresholds defined by standards) or damage, they need to be taken out and replaced and that causes many delays and problems. This would be longer in lighter traffic lines, but in heavy and mostly used traffic lines the rail life is 2-3 years. Surface treatment methods increase the lifetime of rails and coating over rail surface have given good solution for those problems. Laser cladding is an additive manufacturing coating method. It allows the same or a different type of material to be coated over a rail or wheel substrate. Laser cladding process parameters and material selections are important factors for achieving this purpose. In this thesis work showed that laser clad coated rail specimens tested under different test scales: small-scale tests, full-scale tests in laboratory conditions and field tests with actual environmental conditions. Material selection of laser clad specimens was based on previous tests for improved wear and RCF resistance. They were compared with standard grade rails and premium rails. The clad materials were martensitic stainless steel (MSS), Stellite 6, R260, and T400. The substrate rail material used was R260 grade rail. Also, some premium rail tests were conducted for comparison: Manganese (Mn), Chromium (Cr) and R400 HT. Small-scale twin disc tests were conducted to find the full lifespan of MSS clad and some repair solutions with MSS clad, Stellite 6 clad and R260 clad over R260 rail specimen “damage”. The premium rail specimens were analysed and compared with R260 rail specimen and MSS clad specimens. Also, laser cladding process parameters were changed with MSS clad over R260 rail and tested to find how clad “quality” affects the performance of clad specimens and how defects change or cause problems when optimal clad parameters changed. Full-scale tests were conducted to see how clad specimens and repair specimens perform under actual loading conditions. MSS clad, Stellite 6 clad and R260 un-clad pocket specimens were analysed and compared with small scale tests. A T400 rail specimen was tested for repair analysis. The results of small-scale tests were reflected in the full-scale test outcomes. In all tests the clad layers performed well in terms of wear and RCF resistance which gave the confidence needed to initiate field tests. MSS clad twin-disc experiments showed that the clad disc did not fail over 400,000 cycles. However, experiments with R260 standard grade rail discs observed failures occurring around 15,000 cycles in the literature. It is evident that the MSS clad disc exhibited at least 20-25 times higher wear and rolling contact fatigue (RCF) resistance than the standard grade rail disc. These were started, and data collection undertaken for R260 rails, HP 335 premium rails, MSS clad rails with different clad thickness, Stellite 6 clad rails, and insulated block joint (IBJ) components."],"dc:format":["text"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/35352/1/Kazim%20Yildirimli_Scaling%20Up%20The%20Tribological%20Assessment%20of%20Laser%20Clad%20Rail%20to%20Build%20The%20Case%20For%20Field%20Implementation.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Mechanical Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/35352/"],"dc:relation.references":["AbrasiMet 250. (n.d.).“AbrasiMet 250B Brochure.” [Online]. Available at: https://www.buehler.com/assets/Brochures/English/Sectioning/AbrasiMet250Brochure.pdf. Athukorala, A., & De Pellegrin, D. V. (2017). Experimental Depiction of the Hypothesis of Flake-Like Wear Debris Generation in Rolling Contact Fatigue of the Rail–Wheel Contact Interface. Tribology Transactions, 60(4), 581–591. https://doi.org/10.1080/10402004.2016.1188189 Ayrault, S., Chateauminois, A., Soulier, J. P., Tréheux, D., & Vannes, A. B. (1996). Deposition of a ceramic coating on a thermoplastic polymer by atmospheric plasma and laser cladding. Surface and Coatings Technology. https://doi.org/10.1016/0257-8972(95)02432-8 Beaty, P., Temple, B., Marshall, M. B., & Lewis, R. (2015). Experimental modelling of lipping in insulated rail joints and investigation of rail head material improvements. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 230(4), 1375–1387. https://doi.org/10.1177/0954409715600740 Bhadeshia, H., & Honeycombe, R. (2006). Steels: Microstructure and Properties. In Steels: Microstructure and Properties. https://doi.org/10.1016/B978-0-7506-8084-4.X5000-6 Bolton, P. J., & Clayton, P. (1984). Rolling-sliding wear damage in rail and tyre steels. Wear. https://doi.org/10.1016/0043-1648(84)90066-8 Brunskill, H. P., Zhou, L., Lewis, R., Marshall, M. B., & Dwyer-Joyce, R. S. (2012). Dynamic characterisation of the wheel/rail contact using ultrasonic reflectometry. 9th International Conference on Contact Mechanics and Wear of Rail/Wheel Systems, CM 2012, January, 98–102. https://doi.org/10.4203/ccp.104.185 Buckley-Johnstone, L., Harmon, M., Lewis, R., Hardwick, C., & Stock, R. (2019). A comparison of friction modifier performance using two laboratory test scales. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 233(2), 201–210. https://doi.org/10.1177/0954409718787045 Christoforou, P. (2020). Laser Cladding for use in Extreme Tribological Interfaces. Christoforou, P., Fletcher, D. I., & Lewis, R. (2019). Benchmarking of premium rail material wear. Wear, 436–437. https://doi.org/10.1016/j.wear.2019.202990 Christoforou, P., Lewis, S., Fletcher, D. I., Pavier, M. J., Mostafavi, M., Narayanan, A., & Lewis, R. (n.d.). Review of laser cladding tribology for high load applications Review of laser cladding tribology for high load applications. Chryssolouris, G., Zannis, S., Tsirbas, K., & Lalas, C. (n.d.). An Experimental Investigation of Laser Cladding. Chryssolouris, G., Zannis, S., Tsirbas, K., & Lalas, C. (2002). An experimental investigation of laser cladding. CIRP Annals - Manufacturing Technology. https://doi.org/10.1016/S0007-8506(07)61486-3 Clare, A., Olusola, O., Folkes, J., & Farayibi, P. (2011). Laser cladding for railway repair and preventative maintenance. 30th International Congress on Applications of Lasers and Electro-Optics, ICALEO 2011, September 2017, 240–249. https://doi.org/10.2351/1.4710578 Creaform3D. (n.d.). “HandySCAN BLACK 3D Laser Scanner.” [Online]. Available at: https://www.creaform3d.com/en/portable-3d-scanner-handyscan-3d. Cubus. (n.d.). “TestXpert testingsoftware, Cubus Testing software” [Online]. Available at: https://www.zwickroell.com/accessories/testxpert-testing-software/cubus-testing-software/ . DuraScan. (n.d.). “DuraScan micro hardness tester.” [Online]. Available at: http://f.jernindustri.dk/2fk3ntzke7ogxgha.pdf. EcoMet 250. (n.d.). “BUEHLER® EcoMet®250/300 Grinder-Polisher Family & AutoMet®250/300 Power Head.” [Online]. Available at: https://photos.labwrench.com/equipmentManuals/8248-3228.pdf. Ehsan Toyserkani, Amir Khajepour, & Stephen F. Corbin. (2004). Laser Cladding. Fasihi, P., Kendall, O., Abrahams, R., Mutton, P., Qiu, C., Schläfer, T., & Yan, W. (2022). Tribological Properties of Laser Cladded Alloys for Repair of Rail Components. Materials, 15(21), 7466. https://doi.org/10.3390/ma15217466 Fletcher, D. I., & Beynon, J. H. (2000). Development of a Machine for Closely Controlled Rolling Contact Fatigue and Wear Testing. Journal of Testing and Evaluation, 28(4), 267–275. https://doi.org/10.1520/jte12104j Franklin, F. J., Weeda, G. J., Kapoor, A., & Hiensch, E. J. M. (2005). Rolling contact fatigue and wear behaviour of the infrastar two-material rail. Wear, 258(7–8), 1048–1054. https://doi.org/10.1016/j.wear.2004.03.054 Fu, F., Zhang, Y., Chang, G., & Dai, J. (2016). Analysis on the physical mechanism of laser cladding crack and its influence factors. Optik, 127(1), 200–202. https://doi.org/10.1016/j.ijleo.2015.10.043 Fu, Z. K., Ding, H. H., Wang, W. J., Liu, Q. Y., Guo, J., & Zhu, M. H. (2015). Investigation on microstructure and wear characteristic of laser cladding Fe-based alloy on wheel/rail materials. Wear, 330–331, 592–599. https://doi.org/10.1016/j.wear.2015.02.053 Gao, J., Zhai, W., & Guo, Y. (2018). Wheel–rail dynamic interaction due to rail weld irregularity in high-speed railways. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 232(1), 249–261. https://doi.org/10.1177/0954409716664933 Garnham, J. E., & Beynon, J. H. (1991). The early detection of rolling-sliding contact fatigue cracks. In Wear (Vol. 44). Guo, H. ming, Wang, Q., Wang, W. jian, Guo, J., Liu, Q. yue, & Zhu, M. hao. (2015). Investigation on wear and damage performance of laser cladding Co-based alloy on single wheel or rail material. Wear, 328–329, 329–337. https://doi.org/10.1016/j.wear.2015.03.002 Heyder, R., & Maedler, K. (2015). The influence of wheel and rail material on the wear of the respective contact partner. CM 2015 - 10th International Conference on Contact Mechanics of Wheel / Rail Systems. Hitachi. (n.d.). “Hitachi Tabletop Microscope TM3030.” [Online]. Available at: https://www.hitachi-hightech.com/file/us/pdf/library/literature/TM3030_brochure_letter.pdf. HP335. (n.d.). “HP335 Rail for combatting rolling contact fatigue and wear .” [Online]. Available at: https://britishsteel.co.uk/media/323526/british-steel-hp335-datasheet.pdf. HP335. (2020). HP335 Rail for combatting rolling contact fatigue and wear. Hu, Y., Zhou, L., Ding, H. H., Tan, G. X., Lewis, R., Liu, Q. Y., Guo, J., & Wang, W. J. (2020). Investigation on wear and rolling contact fatigue of wheel-rail materials under various wheel/rail hardness ratio and creepage conditions. Tribology International. https://doi.org/10.1016/j.triboint.2019.106091 Hysitron. (n.d.). “Hysitron TS 77 Select Nanoindenter.” [Online]. Available at: https://www.bruker.com/en/products-and-solutions/test-and-measurement/nanomechanical-test-systems/hysitron-ts-77-select-nanoindenter.html. ImageJ. (n.d.). “Image Processing and Analysis” [Online]. Available at: https://imagej.nih.gov/ij/docs/intro.html. InfiniteFocusSL | 3D measurement system for form & finish | Alicona. (n.d.). Retrieved February 17, 2023, from https://www.alicona.com/products/infinitefocussl/ Kaierle, S., Barroi, A., Noelke, C., Hermsdorf, J., Overmeyer, L., & Haferkamp, H. (2012). Review on Laser Deposition Welding: From Micro to Macro. Physics Procedia. https://doi.org/10.1016/j.phpro.2012.10.046 Kendall, O., Abrahams, R., Paradowska, A., Reid, M., Qiu, C., Mutton, P., Schläfer, T., & Yan, W. (2023). Influence of multi-layer laser cladding depositions and rail curvature on residual stress in light rail components. Engineering Failure Analysis, 150. https://doi.org/10.1016/j.engfailanal.2023.107330 Kendall, O., Fasihi, P., Abrahams, R., Paradowska, A., Reid, M., Lai, Q., Qiu, C., Mutton, P., Soodi, M., & Yan, W. (2022). Application of a New Alloy and Post Processing Procedures for Laser Cladding Repairs on Hypereutectoid Rail Components. Materials, 15(15). https://doi.org/10.3390/ma15155447 Kendall, O., Paradowska, A., Abrahams, R., Reid, M., Qiu, C., Mutton, P., & Yan, W. (2023). Residual Stress Measurement Techniques for Metal Joints, Metallic Coatings and Components in the Railway Industry: A Review. In Materials (Vol. 16, Issue 1). MDPI. https://doi.org/10.3390/ma16010232 Lai, Q., Abrahams, R., Yan, W., Qiu, C., Mutton, P., Paradowska, A., Soodi, M., & Wu, X. (2019). Influences of depositing materials, processing parameters and heating conditions on material characteristics of laser-cladded hypereutectoid rails. Journal of Materials Processing Technology, 263, 1–20. https://doi.org/10.1016/j.jmatprotec.2018.07.035 Langford, G., & Sc, D. (2023). Microstructures. 1–5. Lewis, R., Christoforou, P., Wang, W. J., Beagles, A., Burstow, M., & Lewis, S. R. (2019). Investigation of the influence of rail hardness on the wear of rail and wheel materials under dry conditions (ICRI wear mapping project). Wear, 430–431(January), 383–392. https://doi.org/10.1016/j.wear.2019.05.030 Lewis, R., & Dwyer-Joyce, R. S. (2004). Wear mechanisms and transitions in railway wheel steels. In Part J: J. Engineering Tribology (Vol. 218). Lewis, R., & Olofsson, U. (2009). Basic tribology of the wheel-rail contact. In Wheel-Rail Interface Handbook. https://doi.org/10.1533/9781845696788.1.34 Lewis, S. R., Fretwell-Smith, S., Goodwin, P. S., Smith, L., Lewis, R., Aslam, M., Fletcher, D. I., Murray, K., & Lambert, R. (2016a). Improving rail wear and RCF performance using laser cladding. Wear, 366–367, 268–278. https://doi.org/10.1016/j.wear.2016.05.011 Lewis, S. R., Fretwell-Smith, S., Goodwin, P. S., Smith, L., Lewis, R., Aslam, M., Fletcher, D. I., Murray, K., & Lambert, R. (2016b). Improving rail wear and RCF performance using laser cladding. Wear, 366–367, 268–278. https://doi.org/10.1016/j.wear.2016.05.011 Lewis, S. R., Lewis, R., Evans, G., & Buckley-Johnstone, L. E. (2014). Assessment of railway curve lubricant performance using a twin-disc tester. Wear, 314(1–2), 205–212. https://doi.org/10.1016/j.wear.2013.11.033 Lewis, S. R., Lewis, R., & Fletcher, D. I. (2015a). Assessment of laser cladding as an option for repairing/enhancing rails. Wear, 330–331, 581–591. https://doi.org/10.1016/j.wear.2015.02.027 Lewis, S. R., Lewis, R., & Fletcher, D. I. (2015b). Assessment of laser cladding as an option for repairing/enhancing rails. Wear, 330–331, 581–591. https://doi.org/10.1016/j.wear.2015.02.027 Lewis, S. R., Lewis, R., Goodwin, P. S., Fretwell-Smith, S., Fletcher, D. I., Murray, K., & Jaiswal, J. (2017a). Full-scale testing of laser clad railway track; Case study – Testing for wear, bend fatigue and insulated block joint lipping integrity. Wear, 376–377, 1930–1937. https://doi.org/10.1016/j.wear.2017.02.023 Lewis, S. R., Lewis, R., Goodwin, P. S., Fretwell-Smith, S., Fletcher, D. I., Murray, K., & Jaiswal, J. (2017b). Full-scale testing of laser clad railway track; Case study – Testing for wear, bend fatigue and insulated block joint lipping integrity. Wear, 376–377(February), 1930–1937. https://doi.org/10.1016/j.wear.2017.02.023 Lewis, S. R., Lewis, R., Goodwin, P. S., Fretwell-Smith, S., Fletcher, D. I., Murray, K., & Jaiswal, J. (2017c). Full-scale testing of laser clad railway track; Case study – Testing for wear, bend fatigue and insulated block joint lipping integrity. Wear, 376–377(February), 1930–1937. https://doi.org/10.1016/j.wear.2017.02.023 Lu, P., Lewis, S. R., Fretwell-Smith, S., Fletcher, D. I., & Lewis, R. (2018). Laser cladding of rail; The effects of depositing material on lower rail grades. Proceedings of the 11th International Conference on Contact Mechanics and Wear of Rail/Wheel Systems, CM 2018, 610–617. https://doi.org/10.1016/j.wear.2019.203045 Magel, E., Mutton, P., Ekberg, A., & Kapoor, A. (2016). Rolling contact fatigue, wear and broken rail derailments. Wear, 366–367, 249–257. https://doi.org/10.1016/j.wear.2016.06.009 Mandal, N. K. N., & Peach, B. (2010). An Engineering Analysis of Insulated Rail Joints: A General Perspective. International Journal of Engineering Science and Technology, 2(8), 3964–3988. Mansouri, H., & Monshi, A. (2004). Microstructure and residual stress variations in weld zone of flash-butt welded railroads. Science and Technology of Welding and Joining, 9(3). https://doi.org/10.1179/136217104225012201 Markov, D. (1995). Laboratory tests for wear of rail and wheel steels. Wear. https://doi.org/10.1016/0043-1648(95)90184-1 Martensitic Stainless Steels. (n.d.). [Online]. Available at: https://bssa.org.uk/wp-content/uploads/2021/02/Martensitics_JB_2.pdf Microset (n.d.) “General purpose system for small to medium replication and moulding applications.” [Online]. Available at: https://www.microset.co.uk/products/50ml-system/index.html. Narayanan, A., Mostafavi, M., Pirling, T., Kabra, S., Lewis, R., Pavier, M. J., & Peel, M. J. (2019). Residual stress in laser cladded rail. Tribology International, 140(May), 105844. https://doi.org/10.1016/j.triboint.2019.105844 Nellian, A. S., Tan, K. E., Hoh, H. J., Pang, J. H. L., Christian, I., & Chua, S. Y. (2019, February 13). Microstructure and Wear Performance Assessment of Laser Cladded Rail Steel for Service Life Extension at Sharp-Radius Curves. 2018 International Conference on Intelligent Rail Transportation, ICIRT 2018. https://doi.org/10.1109/ICIRT.2018.8641613 Nextsense. (n.d.). “Calipri, Highly Precise Profile Measurement for Predictive Maintenance.” [Online]. Available at: https://www.nextsense-worldwide.com/en/industries/railway.html. Niederhauser, S., & Karlsson, B. (2005). Fatigue behaviour of Co-Cr laser cladded steel plates for railway applications. Wear, 258(7–8), 1156–1164. https://doi.org/10.1016/j.wear.2004.03.026 Nikon. (n.d.). “Eclipse LV150 and LV150A.” [Online]. Available at: https://www.bu.edu/photonics/files/2016/11/Nikon-LV150-Brochure.pdf. Nishikawa, L. P., & Goldenstein, H. (2019). Divorced Eutectoid on Heat-Affected Zone of Welded Pearlitic Rails. JOM, 71(2), 815–823. https://doi.org/10.1007/s11837-018-3213-5 Olofsson, U., Zhu, Y., Abbasi, S., Lewis, R., & Lewis, S. (2013). Tribology of the wheel-rail contact-aspects of wear, particle emission and adhesion. Vehicle System Dynamics, 51(7), 1091–1120. https://doi.org/10.1080/00423114.2013.800215 Pawlowski, L. (1999). Thick laser coatings: A review. Journal of Thermal Spray Technology. https://doi.org/10.1361/105996399770350502 Qian, L., Li, M., Zhou, Z., Yang, H., & Shi, X. (2005). Comparison of nano-indentation hardness to microhardness. Surface and Coatings Technology, 195(2–3), 264–271. https://doi.org/10.1016/j.surfcoat.2004.07.108 Roy, T., Paradowska, A., Abrahams, R., Law, M., Mutton, P., Soodi, M., & Yan, W. (2020). Residual stress in laser cladded heavy-haul rails investigated by neutron diffraction. Journal of Materials Processing Technology, 278. https://doi.org/10.1016/j.jmatprotec.2019.116511 Santa, J. F., Cuervo, P., Christoforou, P., Harmon, M., Beagles, A., Toro, A., & Lewis, R. (2019). Twin disc assessment of wear regime transitions and rolling contact fatigue in R400HT – E8 pairs. Wear, 432–433(January), 102916. https://doi.org/10.1016/j.wear.2019.05.031 Schmid, F., Burstow, M., & Clark, S. (2010). Best Practice in Wheel-rail Interface Management for Mixed Traffic Railways. University of Birmingham Press. https://books.google.co.uk/books?id=YM0hnwEACAAJ SciAps. (n.d.). “Handheld LIBS Analyser -SciAps Z-200+.” [Online]. Available at: https://www.qesnet.com/product/handheld-libs-analyser-sciaps-z-200/. Seo, J. W., Kim, J. –C, Kwon, S. J., & Jun, H. K. (2019). Effects of Laser Cladding for Repairing and Improving Wear of Rails. International Journal of Precision Engineering and Manufacturing, 20(7), 1207–1217. https://doi.org/10.1007/s12541-019-00115-y SF HT. (2017). “SF heat-treated range”. [Online]. Available at: https://uploads-ssl.webflow.com/5db81e2f6c50c20ceba8dc08/5f478fe902f03e69a35e1e32_British%20Steel%20Stress%20Free%20Range%20Data%20Sheet.pdf SimpliMet 1000. (n.d.). “Buehler SimpliMet 1000&3000 Automatic Mounting Press.” [Online]. Available at: http://www.sjstmat.com/uploadfile/2012/0118/20120118121742618.pdf. Singh, R., Kumar, D., Mishra, S. K., & Tiwari, S. K. (2014). Laser cladding of Stellite 6 on stainless steel to enhance solid particle erosion and cavitation resistance. Surface and Coatings Technology. https://doi.org/10.1016/j.surfcoat.2014.04.008 Srisungsitthisunti, P., Kaewprachum, B., Yang, Z., & Gao, G. (2022). Real-Time Quality Monitoring of Laser Cladding Process on Rail Steel by an Infrared Camera. Metals, 12(5). https://doi.org/10.3390/met12050825 StelliteTM, J., & KoteTM, D. (n.d.). “Stellite TM 6 Alloy”. [Online]. Available at: https://www.deloro.com/fileadmin/users/redakteur/006_Downloads/Data_Sheets/Deloro_MDS_Stellite6_rev00.pdf Suh, N. P. (1977). AN OVERVIEW OF THE DEL~INA~ON THEORY OF WEAR. In Wear (Vol. 44). Elsevier Sequoia S.A. Thompson, D. (2009). Railway Noise and Vibration. In Railway Noise and Vibration. https://doi.org/10.1016/B978-0-08-045147-3.X0023-0 Tomlinson, K., Fletcher, D., & Lewis, R. (2021). Measuring material plastic response to cyclic loading in modern rail steels from a minimal number of twin-disc tests: Https://Doi.Org/10.1177/0954409721993615. Toyserkani, E., Khajepour, A., & Corbin, S. (2017). Laser Cladding - A Versatile Proactive and Reactive Technology. New York. https://doi.org/10.2351/1.521888 Tyfour, W. R., Beynon, J. H., & Kapoor, A. (1995). The steady state wear behaviour of pearlitic rail steel under dry rolling-sliding contact conditions. Wear. https://doi.org/10.1016/0043-1648(94)06533-0 University of Southampton. (n.d.). “µ-VIS: Multidisciplinary, Multiscale, Microtomographic Volume Imaging” [Online], Available at: https://www.southampton.ac.uk/muvis/about/equipment/hutch.page. Vilar, R. (2001). Laser cladding. International Journal of Powder Metallurgy (Princeton, New Jersey), 37(2). https://doi.org/10.2351/1.521888 Vishnu, P. R. (2018). Solid-State Transformations in Weldments. In Welding, Brazing, and Soldering. https://doi.org/10.31399/asm.hb.v06.a0001341 Wang, W. J., Hu, J., Guo, J., Liu, Q. Y., & Zhu, M. H. (2014). Effect of laser cladding on wear and damage behaviors of heavy-haul wheel/rail materials. Wear, 311(1–2), 130–136. https://doi.org/10.1016/j.wear.2014.01.011 Wang, X., Lei, L., & Yu, H. (2021). A review on microstructural features and mechanical properties of wheels/rails cladded by laser cladding. Micromachines, 12(2), 1–16. https://doi.org/10.3390/mi12020152 Weng, F., Chen, C., & Yu, H. (2014). Research status of laser cladding on titanium and its alloys: A review. In Materials and Design. https://doi.org/10.1016/j.matdes.2014.01.077 Wesselmecking, S., Haupt, M., Ma, Y., Song, W., Hirt, G., & Bleck, W. (2021). Mechanism-controlled thermomechanical treatment of high manganese steels. Materials Science and Engineering A, 828, 142056. https://doi.org/10.1016/j.msea.2021.142056 Williams, J. (2005). Engineering tribology. In Engineering Tribology. https://doi.org/10.1017/CBO9780511805905 Xiaoyan Zeng, Zengyi Tao, Beidi Zhu, Erhua Zhou, & Kun Cui. (1996). Investigation of laser cladding ceramic-metal composite coatings: processing modes and mechanisms. Surface and Coatings Technology. https://doi.org/10.1016/0257-8972(95)02431-x Xie, T., Zhou, L., Ding, H., Zhu, Y., Yang, W., Xiao, Q., Wang, W., Guo, J., & Liu, Q. (2021). Investigation on the rolling contact fatigue behaviors of different laser cladding materials on the damaged rail. Journal of Tribology, 143(5), 1–13. https://doi.org/10.1115/1.4050690 Xin, L., Markine, V., & Shevtsov, I. (2018). Analysis of the effect of repair welding/grinding on the performance of railway crossings using field measurements and finite element modeling. Proceedings of the Institution of Mechanical Engineers, Part F: Journal of Rail and Rapid Transit, 232(3), 798–815. https://doi.org/10.1177/0954409717693960 Ya, W. (2015). Laser Materials Interactions During a Nalyses on Clad Formation , Thermal Cycles , Residual. Zanzarin, S. (2015). Laser Cladding with metallic powders. University of Trento, November, 133. Zhang, B., He, B., & Wang, H. (2022). Microstructural investigation and mechanical performance of laser cladding repaired bainite steel with AerMet100 steel. Surface and Coatings Technology, 440(April), 128498. https://doi.org/10.1016/j.surfcoat.2022.128498 Zhu, D., Wang, J., & Wang, Q. J. (2015). On the Stribeck Curves for Lubricated Counterformal Contacts of Rough Surfaces. Journal of Tribology, 137(2). https://doi.org/10.1115/1.4028881 Zhu, Y., Wang, W., Lewis, R., Yan, W., Lewis, S. R., & Ding, H. (2019). A review on wear between railway wheels and rails under environmental conditions. In Journal of Tribology (Vol. 141, Issue 12). American Society of Mechanical Engineers (ASME). https://doi.org/10.1115/1.4044464 Zhu, Y., Yang, Y., Mu, X., Wang, W., Yao, Z., & Yang, H. (2019). Study on wear and RCF performance of repaired damage railway wheels: Assessing laser cladding to repair local defects on wheels. Wear. https://doi.org/10.1016/j.wear.2019.04.028"],"dcterms:accessrights":["public"],"dc:title":["Scaling Up The Tribological Assessment of Laser Clad Rail to Build The Case For Field Implementation"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"],"person:identifier.orcid":["0000000177398342"]},"updated_at":"2026-11-18T23:27:24Z"}