{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:35611"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:35611","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Doping Mechanisms and Electrical Properties of Sodium Niobate","abstract":"Intermediate temperature solid oxide fuel cells (ITSOFCs) are one of many technologies attempting to decarbonise global energy production and utilise the hydrogen economy. Unfortunately, typical solid oxide electrolytes such as yttria-stabilised zirconia (YSZ) do not exhibit sufficient conductivity for operation in the intermediate temperature region (400-750 °C). As a result, many potential intermediate temperature solid oxide electrolytes have undergone investigation to replace YSZ. The goal of this project was to investigate the perovskite material NaNbO3 (NN) and identify its suitability as a solid oxide electrolyte. NN ceramics were prepared via solid-state reaction of mixed oxides at 900 °C, followed by sintering at temperatures in the range 1240-1350 °C. Physical properties of NN ceramics were assessed using X-Ray diffraction (XRD), Scanning Electron Microscopy (SEM), Electron Probe Micro Analysis (EPMA) and Nuclear Magnetic Resonance (NMR). Electrical properties were investigated using impedance spectroscopy to assess bulk conductivity and pO2 dependence of the ceramics, probostat measurements have allowed for determination of oxygen ion transport numbers (tion) and the electronic band gap of NN has been determined via UV-Vis spectroscopy. This project is divided into exploring the defect chemistry of NN and how it influences the electrical properties. It has been shown that NN produced via solid-state synthesis varies significantly compared to hydrothermally prepared, and commercially available NN powders. The variance has been attributed to non-stoichiometry between the sodium and niobium sites caused by sodium volatility during processing. Deliberate Na:Nb non-stoichiometry in the range 0.96-1.22 showcases that sodium rich NN exhibits greater bulk conductivities (55:45 NN σ500°C ≈ 26 μS cm-1) and promotes ionic conductivity, compared to sodium deficient NN (49:51 NN σ500°C ≈ 0.13 μS cm-1). The following doping mechanisms have been used to influence the electrical properties of NN: 1. Direct substitution of sodium for calcium to generate A-site vacancies: 2Na+ = Ca2+ 2. A-site donor doping using Mg2+ and Ga3+ for the reduction of oxygen vacancies: Na+ = Mg2+ + 0.5O2- 3. B-site donor doping using W6+ and Mo6+ for the reduction of oxygen vacancies: Nb5+ = W6+ + 0.5O2- 4. B-site acceptor doping using Mg2+, Ga3+ and Ti4+ for the generation of oxygen vacancies: Nb5+ + O2- = Ga3+ Generation of A-site vacancies via calcium doping leads to an increase in bulk conductivity (Na0.9Ca0.05NbO3 σ500°C ≈ 2.7 μS cm-1), with low levels of ionic conductivity attributed to sodium ion conduction. Donor doping of the A-site using Mg2+ or Ga3+ has no significant effect on the bulk conductivity (Na0.99Mg0.01NbO3.005 σ500°C ≈ 0.24 μS cm-1), however, ionic conductivity is supressed. Similarly, donor doping the B-site with W6+ supresses ionic conductivity without influencing bulk conductivity (NaNb0.99W0.01O3.005 σ500 °C ≈ 0.69 μS cm-1). However, doping with molybdenum does not appear to be successful due to preferential formation of a molybdenum bronze. Acceptor doping of the B-site with Ga3+ and Ti4+ promotes ionic conductivity and greatly enhances bulk conductivity (NaNb0.95Ga0.05O2.95 σ500 °C ≈ 0.08 mS cm-1/NaNb0.95Ti0.05O2.975 σ500 °C ≈ 0.05 mS cm-1). It has been shown that in gallium doped NN maximum conductivities are achieved at very low concentrations (<1at%) of dopant due to pinning of oxygen vacancies. Acceptor doping with Mg2+ appears to be unsuccessful due to a preference for A-site donor doping. The properties of NN vary significantly according to the dopant mechanism utilised, and the Na:Nb ratio. The electronic band gap of NN appears to be unaffected by acceptor doping and remains 3.4 eV. Oxygen ion transport numbers for acceptor doped NN ceramics indicate that all variants are mixed oxide ion-electronic conductors (tion=0.2-0.7), indicating that NN based materials are unsuitable for applications as solid oxide electrolytes.","abstract_html":"Intermediate temperature solid oxide fuel cells (ITSOFCs) are one of many technologies attempting to decarbonise global energy production and utilise the hydrogen economy. Unfortunately, typical solid oxide electrolytes such as yttria-stabilised zirconia (YSZ) do not exhibit sufficient conductivity for operation in the intermediate temperature region (400-750 °C). As a result, many potential intermediate temperature solid oxide electrolytes have undergone investigation to replace YSZ. The goal of this project was to investigate the perovskite material NaNbO3 (NN) and identify its suitability as a solid oxide electrolyte. NN ceramics were prepared via solid-state reaction of mixed oxides at 900 °C, followed by sintering at temperatures in the range 1240-1350 °C. Physical properties of NN ceramics were assessed using X-Ray diffraction (XRD), Scanning Electron Microscopy (SEM), Electron Probe Micro Analysis (EPMA) and Nuclear Magnetic Resonance (NMR). Electrical properties were investigated using impedance spectroscopy to assess bulk conductivity and pO2 dependence of the ceramics, probostat measurements have allowed for determination of oxygen ion transport numbers (tion) and the electronic band gap of NN has been determined via UV-Vis spectroscopy. This project is divided into exploring the defect chemistry of NN and how it influences the electrical properties. It has been shown that NN produced via solid-state synthesis varies significantly compared to hydrothermally prepared, and commercially available NN powders. The variance has been attributed to non-stoichiometry between the sodium and niobium sites caused by sodium volatility during processing. Deliberate Na:Nb non-stoichiometry in the range 0.96-1.22 showcases that sodium rich NN exhibits greater bulk conductivities (55:45 NN σ500°C ≈ 26 μS cm-1) and promotes ionic conductivity, compared to sodium deficient NN (49:51 NN σ500°C ≈ 0.13 μS cm-1). The following doping mechanisms have been used to influence the electrical properties of NN: 1. Direct substitution of sodium for calcium to generate A-site vacancies: 2Na+ = Ca2+ 2. A-site donor doping using Mg2+ and Ga3+ for the reduction of oxygen vacancies: Na+ = Mg2+ + 0.5O2- 3. B-site donor doping using W6+ and Mo6+ for the reduction of oxygen vacancies: Nb5+ = W6+ + 0.5O2- 4. B-site acceptor doping using Mg2+, Ga3+ and Ti4+ for the generation of oxygen vacancies: Nb5+ + O2- = Ga3+ Generation of A-site vacancies via calcium doping leads to an increase in bulk conductivity (Na0.9Ca0.05NbO3 σ500°C ≈ 2.7 μS cm-1), with low levels of ionic conductivity attributed to sodium ion conduction. Donor doping of the A-site using Mg2+ or Ga3+ has no significant effect on the bulk conductivity (Na0.99Mg0.01NbO3.005 σ500°C ≈ 0.24 μS cm-1), however, ionic conductivity is supressed. Similarly, donor doping the B-site with W6+ supresses ionic conductivity without influencing bulk conductivity (NaNb0.99W0.01O3.005 σ500 °C ≈ 0.69 μS cm-1). However, doping with molybdenum does not appear to be successful due to preferential formation of a molybdenum bronze. Acceptor doping of the B-site with Ga3+ and Ti4+ promotes ionic conductivity and greatly enhances bulk conductivity (NaNb0.95Ga0.05O2.95 σ500 °C ≈ 0.08 mS cm-1/NaNb0.95Ti0.05O2.975 σ500 °C ≈ 0.05 mS cm-1). It has been shown that in gallium doped NN maximum conductivities are achieved at very low concentrations (&lt;1at%) of dopant due to pinning of oxygen vacancies. Acceptor doping with Mg2+ appears to be unsuccessful due to a preference for A-site donor doping. The properties of NN vary significantly according to the dopant mechanism utilised, and the Na:Nb ratio. The electronic band gap of NN appears to be unaffected by acceptor doping and remains 3.4 eV. Oxygen ion transport numbers for acceptor doped NN ceramics indicate that all variants are mixed oxide ion-electronic conductors (tion=0.2-0.7), indicating that NN based materials are unsuitable for applications as solid oxide electrolytes.","abstract_has_math":false,"creators":["Canton, Jordan"],"institution":"University of Sheffield","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Sinclair, Derek"],"committee_chairs":[],"committee_members":[],"year":2024,"date_issued":"2024-03","date_published":"2024-03","updated_at":"2026-11-18T23:27:55Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["2375383","ICASE"],"render_values":[{"text":"2375383","href":null,"code":true},{"text":"ICASE","href":null,"code":true}]}],"person_identifier_entries":[{"key":"person:identifier.orcid","label":"ORCID","values":["0009000590977513"],"render_values":[{"text":"0009-0005-9097-7513","href":"https://orcid.org/0009-0005-9097-7513","code":true}]}]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/35611/1/Jordan%20Canton%20-%20Doping%20Mechanisms%20and%20Electrical%20Properties%20of%20Sodium%20Niobate.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A35611","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Sinclair, Derek"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["UKRI","Johnson Matthey"]},{"key":"dc:creator","label":"Author","values":["Canton, Jordan"]},{"key":"person:identifier.orcid","label":"ORCID","values":["0009000590977513"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2024-03"]},{"key":"dc:date.issued","label":"Date","values":["2024-03"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Faculty of Engineering (Sheffield)","Materials Science and Engineering (Sheffield)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Sheffield"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/35611/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["1. Ritchie, H. & Roser, M. Fossil fuels. Our World Data (2017). 2. Maslin, M. Global warming: a very short introduction. (OUP Oxford, 2008). 3. Shafiee, S. & Topal, E. When will fossil fuel reserves be diminished? Energy Policy 37, 181–189 (2009). 4. Iwata, H. & Okada, K. Greenhouse gas emissions and the role of the Kyoto Protocol. Environ. Econ. Policy Stud. 16, 325–342 (2014). 5. Murdock, H. E. Renewables 2019 Global Status Report Collaborative. (2019). 6. Whittingham, M. S. History, evolution, and future status of energy storage. Proc. IEEE 100, 1518–1534 (2012). 7. Marbán, G. & Valdés-Solís, T. Towards the hydrogen economy? Int. J. Hydrogen Energy 32, 1625–1637 (2007). 8. Xu, J. & Froment, G. F. Methane steam reforming, methanation and water‐gas shift: I. Intrinsic kinetics. AIChE J. 35, 88–96 (1989). 9. Stojić, D. L., Marčeta, M. P., Sovilj, S. P. & Miljanić, Š. S. Hydrogen generation from water electrolysis - Possibilities of energy saving. J. Power Sources 118, 315–319 (2003). 10. Vaghari, H., Jafarizadeh-Malmiri, H., Berenjian, A. & Anarjan, N. Recent advances in application of chitosan in fuel cells. Sustain. Chem. Process. 1, 16 (2013). 11. Grove, W. R. XXIV. On voltaic series and the combination of gases by platinum . London, Edinburgh, Dublin Philos. Mag. J. Sci. 14, 127–130 (1839). 12. Grove, W. R. On a gaseous voltaic battery. J. Franklin Inst. 35, 277–280 (1843). 13. Sealy, C. The problem with platinum. Mater. Today 11, 65–68 (2008). 14. Aguiar, P., Adjiman, C. S. & Brandon, N. P. Anode-supported intermediate temperature direct internal reforming solid oxide fuel cell. I: Model-based steady-state performance. J. Power Sources 138, 120–136 (2004). 15. Pei, P., Korom, S. F., Ling, K. & Nasah, J. Cost comparison of syngas production from natural gas conversion and underground coal gasification. Mitig. Adapt. Strateg. Glob. Chang. 21, 629–643 (2016). 16. Pritchard, D. F. & Rattigan, W. M. Hazards of liquid hydrogen: Position paper. 42 (2010). 17. Aloui, T. & Halouani, K. Analytical modeling of polarizations in a solid oxide fuel cell using biomass syngas product as fuel. Appl. Therm. Eng. 27, 731–737 (2007). 18. Minh, N. Q. Ceramic fuel cells. J. Am. Ceram. Soc. 76, 563–588 (1993). 19. Yang, Z., Xia, G. G., Li, X. H. & Stevenson, J. W. (Mn,Co)3O4 spinel coatings on ferritic stainless steels for SOFC interconnect applications. Int. J. Hydrogen Energy 32, 3648–3654 (2007). 20. Zhu, T., Fowler, D. E., Poeppelmeier, K. R., Han, M. & Barnett, S. A. Hydrogen Oxidation Mechanisms on Perovskite Solid Oxide Fuel Cell Anodes. J. Electrochem. Soc. 163, F952–F961 (2016). 21. Hibino, T., Wang, S., Kakimoto, S. & Sano, M. One-chamber solid oxide fuel cell constructed from a YSZ electrolyte with a Ni anode and LSM cathode. Solid State Ionics 127, 89–98 (2000). 22. Benjamin, T. G., Camara, E. H. & Marianowski, L. G. Handbook of fuel cell performance. (1980). 23. Yokokawa, H., Sakai, N., Horita, T. & Yamaji, K. Recent developments in solid oxide fuel cell materials. Fuel cells 1, 117–131 (2001). 24. Yang, Z., Weil, K. S., Paxton, D. M. & Stevenson, J. W. Selection and Evaluation of Heat-Resistant Alloys for SOFC Interconnect Applications. J. Electrochem. Soc. 150, A1188 (2003). 25. Zouhri, K., Shinneeb, M., Chikhalsouk, M. & Cress, J. Solid oxide fuel cell cathode diffusion polarization: materials and exergy study. Energy Convers. Manag. 231, 113865 (2021). 26. Zouhri, K., Shinneeb, M., Chikhalsouk, M. & Cress, J. Solid oxide fuel cell cathode diffusion polarization: materials and exergy study. Energy Convers. Manag. 231, 113865 (2021). 27. Huang, K., Zampieri, A. & Ise, M. Cathode Polarizations of a Cathode-Supported Solid Oxide Fuel Cell. J. Electrochem. Soc. 157, B1471 (2010). 28. Takeguchi, T., Kikuchi, R., Yano, T., Eguchi, K. & Murata, K. Effect of precious metal addition to Ni-YSZ cermet on reforming of CH 4 and electrochemical activity as SOFC anode. Catal. Today 84, 217–222 (2003). 29. Tao, S. & Irvine, J. T. S. A redox-stable efficient anode for solid-oxide fuel cells. Nat. Mater. 2, 320–323 (2003). 30. Zhe, Y., Qizhao, L. & Zhu, B. Thermodynamic analysis of ITSOFC hybrid system for polygenerations. Int. J. Hydrogen Energy 35, 2824–2828 (2010). 31. Shen, J. P. & Song, C. Influence of preparation method on performance of Cu/Zn-based catalysts for low-temperature steam reforming and oxidative steam reforming of methanol for H2 production for fuel cells. Catal. Today 77, 89–98 (2002). 32. Basagiannis, A. C., Panagiotopoulou, P. & Verykios, X. E. Low temperature steam reforming of ethanol over supported noble metal catalysts. Top. Catal. 51, 2–12 (2008). 33. Vivanpatarakij, S., Aiouache, F. & Assabumrungrat, S. Performance of an improved combination unit of Pd-membrane methane steam reformer and intermediate temperature solid oxide fuel cell (C-Pd-ITSOFC). Int. J. Hydrogen Energy 40, 1894–1901 (2015). 34. Brett, D. J. L., Atkinson, A., Brandon, N. P. & Skinner, S. J. Intermediate temperature solid oxide fuel cells. Chem. Soc. Rev. 37, 1568–1578 (2008). 35. Kwon, O. H. & Choi, G. M. Electrical conductivity of thick film YSZ. Solid State Ionics 177, 3057–3062 (2006). 36. Sammes, N. M. & Zhihong, C. Ionic conductivity of ceria/yttria stabilized zirconia electrolyte materials. Solid State Ionics 100, 39–44 (1997). 37. Han, M., Tang, X., Yin, H. & Peng, S. Fabrication, microstructure and properties of a YSZ electrolyte for SOFCs. J. Power Sources 165, 757–763 (2007). 38. Jasinski, P., Petrovsky, V., Suzuki, T., Petrovsky, T. & Anderson, H. U. Electrical Properties of YSZ Films Prepared by Net Shape Technology. J. Electrochem. Soc. 152, A454 (2005). 39. Ishigaki, T., Yamauchi, S., Kishio, K., Mizusaki, J. & Fueki, K. Diffusion of oxide ion vacancies in perovskite-type oxides. J. Solid State Chem. 73, 179–187 (1988). 40. Esaka, T. Oxide Ion Conduction via Interstitial Sites in the Substituted Scheelite-and Spinel-type Oxides. Electrochemistry 78, 16–22 (2010). 41. Zhu, B. Functional ceria-salt-composite materials for advanced ITSOFC applications. J. Power Sources 114, 1–9 (2003). 42. Zhu, B., Fan, L. & Lund, P. Breakthrough fuel cell technology using ceria-based multi-functional nanocomposites. Appl. Energy 106, 163–175 (2013). 43. Gil, V., Moure, C. & Tartaj, J. Sinterability, microstructures and electrical properties of Ni/Gd-doped ceria cermets used as anode materials for SOFCs. J. Eur. Ceram. Soc. 27, 4205–4209 (2007). 44. Lacorre, P., Goutenoire, F., Bohnke, O., Retoux, R. & Laligant, Y. Designing fast oxide-ion conductors. Nature 404, 9–11 (2000). 45. Goutenoire, F., Isnard, O., Retoux, R. & Lacorre, P. Crystal structure of La2Mo2O9, a new fast oxide-ion conductor. Chem. Mater. 12, 2575–2580 (2000). 46. Georges, S. et al. The LAMOX Family of Fast Oxide-Ion Conductors: Overview and Recent Results. J. New Mater. Electrochem. Syst. 7, 51–57 (2004). 47. Evans, I. R., Howard, J. A. K. & Evans, J. S. O. The Crystal Structure of α-La2Mo2O9 and the Structural Origin of the Oxide Ion Migration Pathway. Chem. Mater. 17, 4074–4077 (2005). 48. Le, M. V., Tsai, D. S. & Nguyen, T. A. BSCF/GDC as a refined cathode to the single-chamber solid oxide fuel cell based on a LAMOX electrolyte. Ceram. Int. 44, 1726–1730 (2018). 49. Yokokawa, H. Understanding Materials Compatibility. Annu. Rev. Mater. Res. 33, 581–610 (2003). 50. Mitchell, R. H. Perovskites Modern and Ancient. (2002). 51. Megaw, H. D. Crystal structure of double oxides of the perovskite type. Proc. Phys. Soc. 58, 133–152 (1946). 52. Howard, C. J. & Stokes, H. T. Group-theoretical analysis of octahedral tilting in perovskites. Acta Crystallogr. Sect. B Struct. Sci. 54, 782–789 (1998). 53. Glazer, A. M. The classification of tilted octahedra in perovskites. Acta Crystallogr. Sect. B Struct. Crystallogr. Cryst. Chem. 28, 3384–3392 (1972). 54. Ishihara, T., Matsuda, H. & Takita, Y. Doped LaGaO3 Perovskite Type Oxide as a New Oxide Ionic Conductor. J. Am. Chem. Soc. 116, 3801–3803 (1994). 55. Huang, P. Superior Oxygen Ion Conductivity of Lanthanum Gallate Doped with Strontium and Magnesium. J. Electrochem. Soc. 143, 1644 (1996). 56. Huang, P., Horky, A. & Petric, A. Interfacial reaction between nickel oxide and lanthanum gallate during sintering and its effect on conductivity. J. Am. Ceram. Soc. 82, 2402–2406 (1999). 57. Fergus, J. W. Electrolytes for solid oxide fuel cells. J. Power Sources 162, 30–40 (2006). 58. Li, M. et al. A family of oxide ion conductors based on the ferroelectric perovskite Na0.5Bi0.5TiO3. Nat. Mater. 13, 31–35 (2014). 59. Yang, F. et al. Defect chemistry and electrical properties of sodium bismuth titanate perovskite. J. Mater. Chem. A 6, 5243–5254 (2018). 60. Lu, Y., López, C. A., Wang, J., Alonso, J. A. & Sun, C. Insight into the structure and functional application of Mg-doped Na0.5Bi0.5TiO3 electrolyte for solid oxide fuel cells. J. Alloys Compd. 752, 213–219 (2018). 61. Shafer, M. W. & Roy, R. Phase equilibria in the system Na2O–Nb2O5. J. Am. Ceram. Soc. 42, 482–486 (1959). 62. Egerton, L. & Dillon, D. M. Piezoelectric and dielectric properties of ceramics in the system potassium—sodium niobate. J. Am. Ceram. Soc. 42, 438–442 (1959). 63. Li, P. et al. Mechanism of significantly enhanced piezoelectric performance and stability in textured potassium-sodium niobate piezoelectric ceramics. J. Eur. Ceram. Soc. 38, 75–83 (2018). 64. Megaw, H. D. The Seven Phases of Sodium Niobate. Ferroelectrics 7, 87–89 (1974). 65. Cross, L. E. & Nicholson, B. J. LV. The optical and electrical properties of single crystals of sodium niobate. London, Edinburgh, Dublin Philos. Mag. J. Sci. 46, 453–466 (1955). 66. Reznichenko, L. A. et al. Structural instabilities, incommensurate modulations and P and Q phases in sodium niobate in the temperature range 300-500 K. Crystallogr. Reports 48, 448–456 (2003). 67. Wang, X. B. et al. High temperature Raman study of phase transitions in antiferroelectric NaNbO3. J. Mol. Struct. 385, 1–6 (1996). 68. Glazer, A. M. & Megaw, H. D. Studies of the lattice parameters and domains in the phase transitions of NaNbO3. Acta Crystallogr. Sect. A 29, 489–495 (1973). 69. Zhang, M. H., Fulanović, L., Zhao, C. & Koruza, J. Review on field-induced phase transitions in lead-free NaNbO3-based antiferroelectric perovskite oxides for energy storage. J. Mater. 9, 1–18 (2023). 70. Liu, W., Zhao, D. & Li, S. Large electrostrain with good temperature stability in sodium niobate based ceramics. RSC Adv. 7, 2550–2554 (2017). 71. Wu, J., Xiao, D. & Zhu, J. Potassium-sodium niobate lead-free piezoelectric materials: Past, present, and future of phase boundaries. Chem. Rev. 115, 2559–2595 (2015). 72. Zhang, H., Yang, B., Yan, H. & Abrahams, I. Isolation of a ferroelectric intermediate phase in antiferroelectric dense sodium niobate ceramics. Acta Mater. 179, 255–261 (2019). 73. Shao, T. et al. Potassium-sodium niobate based lead-free ceramics: novel electrical energy storage materials. J. Mater. Chem. A 5, 554–563 (2017). 74. Yang, Z. et al. Significantly enhanced recoverable energy storage density in potassium-sodium niobate-based lead free ceramics. J. Mater. Chem. A 4, 13778–13785 (2016). 75. Luo, N. et al. Well-defined double hysteresis loop in NaNbO3 antiferroelectrics. Nat. Commun. 14, 1776 (2023). 76. Zhang, M. H. et al. Electric-field-induced antiferroelectric to ferroelectric phase transition in polycrystalline NaNbO3. Acta Mater. 200, 127–135 (2020). 77. Tan, X., Ma, C., Frederick, J., Beckman, S. & Webber, K. G. The antiferroelectric ↔ ferroelectric phase transition in lead-containing and lead-free perovskite ceramics. J. Am. Ceram. Soc. 94, 4091–4107 (2011). 78. Zhang, M.-H. et al. Tailoring high-energy storage NaNbO3-based materials from antiferroelectric to relaxor states. Nat. Commun. 2023 141 14, 1–11 (2023). 79. Levin, I. et al. Displacive Order–Disorder Behavior and Intrinsic Clustering of Lattice Distortions in Bi-Substituted NaNbO3. Adv. Funct. Mater. 2001840, 1–13 (2020). 80. Lei, X. et al. Realizing oxygen ion conduction in perovskite structure NaNbO3 by A-site Bismuth doping. J. Alloys Compd. 924, 2–6 (2022). 81. Gouget, G. et al. High Ionic Conductivity in Oxygen-Deficient Ti-Substituted Sodium Niobates and the Key Role of Structural Features. Chem. Mater. 31, 2828–2841 (2019). 82. Gouget, G. et al. Associating and Tuning Sodium and Oxygen Mixed-Ion Conduction in Niobium-Based Perovskites. Adv. Funct. Mater. 30, 1–12 (2020). 83. Zhang, Z. T., Sridhar, S. & Cho, J. W. An investigation of the evaporation of B2O3 and Na2O in f-free mold slags. ISIJ Int. 51, 80–87 (2011). 84. Lee, Y. H., Cho, J. H., Kim, B. I. & Choi, D. K. Piezoelectric properties and densification based on control of volatile mass of potassium and sodium in (K0.5Na0.5)NbO3 ceramics. Jpn. J. Appl. Phys. 47, 4620–4622 (2008). 85. Shimizu, H., Kobayashi, K., Mizuno, Y. & Randall, C. A. Advantages of low partial pressure of oxygen processing of alkali niobate: NaNbO3. J. Am. Ceram. Soc. 97, 1791–1796 (2014). 86. Ferrarelli, M. C., Nuzhnyy, D., Sinclair, D. C. & Kamba, S. Soft-mode behavior and incipient ferroelectricity in Na1/2 Bi1/2 Cu3 Ti4 O12. Phys. Rev. B - Condens. Matter Mater. Phys. 81, 1–7 (2010). 87. Samara, G. A. The relaxational properties of compositionally disordered ABO3 perovskites. J. Phys. Condens. Matter 15, (2003). 88. Kamba, S. et al. Ferroelectric and incipient ferroelectric properties of a novel Sr 9-xPbxCe2Ti2O36(x = 0-9) ceramic system. Chem. Mater. 21, 811–819 (2009). 89. Tagantsev, A. K., Sherman, V. O., Astafiev, K. F., Venkatesh, J. & Setter, N. Ferroelectric materials for microwave tunable applications. J. electroceramics 11, 5–66 (2003). 90. Yadav, A., Pyare, R., Goodenough, J. B. & Singh, P. KTa1- x- yTixGeyO3-δ: A High κ Relaxor Dielectric and Superior Oxide-Ion Electrolyte for IT-SOFC. ACS Appl. Energy Mater. 3, 3205–3211 (2020). 91. Tsvetkov, D. S., Sereda, V. V., Malyshkin, D. A., Ivanov, I. L. & Zuev, A. Y. Chemical lattice strain in nonstoichiometric oxides: an overview. J. Mater. Chem. A 10, 6351–6375 (2022). 92. Gao, R. et al. Designing Optimal Perovskite Structure for High Ionic Conduction. Adv. Mater. 32, 1–9 (2020). 93. Fresno, F. et al. CO2 reduction over NaNbO3 and NaTaO3 perovskite photocatalysts. Photochem. Photobiol. Sci. 16, 17–23 (2017). 94. Handoko, A. D. & Goh, G. K. L. Hydrothermal synthesis of sodium potassium niobate solid solutions at 200 °C. Green Chem. 12, 680–68 (2010). 95. Van Hoek, C. & Koolwijk, M. Conventional wavelength dispersive spectroscopy versus parallel beam spectroscopy - A basic overview. Microchim. Acta 161, 287–293 (2008). 96. Makuła, P., Pacia, M. & Macyk, W. How To Correctly Determine the Band Gap Energy of Modified Semiconductor Photocatalysts Based on UV-Vis Spectra. J. Phys. Chem. Lett. 9, 6814–6817 (2018). 97. Jonscher, A. K. Dielectric relaxation in solids. J. Phys. D. Appl. Phys. 32, R57 (1999). 98. Sinclair, D. C. Characterization of Electro-materials using ac Impedance Spectroscopy. Bol. la Soc. Esp. Ceram. y Vidr. 65, 55–66 (1995). 99. Bruncková, H., Medvecký, L. & Hvizdoš, P. Effect of substrate on phase formation and surface morphology of sol-gel lead-free KNbO3, NaNbO3, and K0.5Na 0.5NbO3 thin films. Chem. Pap. 66, 748–756 (2012). 100. Lee, S., Liu, Z. K., Kim, M. H. & Randall, C. A. Influence of nonstoichiometry on ferroelectric phase transition in BaTiO3. J. Appl. Phys. 101, 1–8 (2007). 101. Ruf, T. et al. The influence on sintering and properties of sodium niobate (NaNbO 3 ) ceramics by “non-stoichiometric” precursor compositions. Mater. Chem. Phys. 229, 437–447 (2019). 102. Shakhovoy, R. A. et al. Ferroelectric Q and antiferroelectric P phases’ coexistence and local phase transitions in oxygen-deficient NaNbO3 single crystal: Micro-Raman, dielectric and dilatometric studies. J. Raman Spectrosc. 43, 1141–1145 (2012). 103. Irvine, J. T. S., Sinclair, D. C. & West, A. R. Electroceramics: Characterization by Impedance Spectroscopy. Adv. Mater. 2, 132–138 (1990). 104. Guo, H., Shimizu, H., Mizuno, Y. & Randall, C. A. Strategy for stabilization of the antiferroelectric phase (Pbma) over the metastable ferroelectric phase (P21ma) to establish double loop hysteresis in lead-free (1-x)NaNbO3-x SrZrO3 solid solution. J. Appl. Phys. 117, 214103 (2015). 105. Masó, N., Woodward, D. I., Várez, A. & West, A. R. Polymorphism, structural characterisation and electrical properties of Na2Nb4O11. J. Mater. Chem. 21, 12096–12102 (2011). 106. Romeu, M. C. et al. Impedance spectroscopy study of TiO2 addition on the ceramic matrix Na2Nb4O11. J. Mater. Sci. Mater. Electron. 24, 4993–4999 (2013). 107. Näfe, H., Amin, R. & Aldinger, F. Thermodynamic Characterization of the Eutectic Phase Mixture NaNbO3/Na3NbO4. II: Solid-State Electrochemical Investigation. J. Am. Ceram. Soc. 90, 3227–3232 (2007). 108. Liu, W. Dielectric and sintering properties of NaNbO3 ceramic prepared by Pechini method. J. Electroceramics 31, 376–381 (2013). 109. Lee, B.-K., Chung, S.-Y. & Kang, S.-J. L. Grain boundary faceting and abnormal grain growth in BaTiO3. Acta Mater. 48, 1575–1580 (2000). 110. Aso, S., Matsuo, H. & Noguchi, Y. Reversible electric-field-induced phase transition in Ca-modified NaNbO3 perovskites for energy storage applications. Sci. Rep. 13, 1–10 (2023). 111. Shannon, R. D. Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Crystallogr. Sect. A Cryst. physics, diffraction, Theor. Gen. Crystallogr. 32, 751–767 (1976). 112. Valant, M. et al. The origin of magnetism in Mn-doped SrTiO 3. Adv. Funct. Mater. 22, 2114–2122 (2012). 113. Choudhury, D. et al. Tuning of dielectric properties and magnetism of SrTiO3 by site-specific doping of Mn. Phys. Rev. B - Condens. Matter Mater. Phys. 84, (2011). 114. Tkach, A., Vilarinho, P. M. & Kholkin, A. L. Polar behavior in Mn-doped SrTiO3 ceramics. Appl. Phys. Lett. 86, 1–3 (2005). 115. Ren, P. et al. Mixed oxide ion and proton conduction and p-type semiconduction in BaTi0.98Ca0.02O2.98 ceramics. J. Mater. Chem. C 1, 2426–2432 (2013). 116. Shi, H., Lu, M., Lan, B. & Zhang, C. Effects of (Mo/W, N) codoping on electronic structures of NaNbO3 based on hybrid density functional calculations. Mod. Phys. Lett. B 32, 1–10 (2018). 117. Roth, R. S. & Waring, J. L. Phase equilibria as related to crystal structure in the system niobium pentoxide-tungsten trioxide. J. Res. Natl. Bur. Stand. Sect. A Phys. Chem. 70A, 281 (1966). 118. West, A. R. Basic Solid State Chemistry. (John Wiley & Sons, Ltd, 1999). 119. Dickens, P. G. & Whittingham, M. S. The tungsten bronzes and related compounds. Q. Rev. Chem. Soc. 22, 30–44 (1968). 120. Wold, A., Kunnmann, W., Arnott, R. J. & Ferretti, A. Preparation and Properties of Sodium and Potassium Molybdenum Bronze Crystals. Inorg. Chem. 3, 545–547 (1964). 121. Ananta, S., Brydson, R. & Thomas, N. W. Synthesis, formation and Characterisation of MgNb2O6 Powder in a Columbite-like Phase. J. Eur. Ceram. Soc. 19, 355–362 (1999). 122. Yang, F., Wu, P. & Sinclair, D. C. Electrical conductivity and conduction mechanisms in (Na0.5Bi0.5TiO3)1−x(BiScO3)x (0.00 ≤ x ≤ 0.25) solid solutions. J. Mater. Chem. C 6, 11598–11607 (2018). 123. Bottelberghs, P. H. & Everts, E. Charge carriers and dc polarization phenomena in solid Na2WO4. J. Solid State Chem. 14, 342–348 (1975). 124. Groszewicz, P. B. et al. The fate of aluminium in (Na,Bi)TiO3-based ionic conductors. J. Mater. Chem. A 8, 18188–18197 (2020). 125. Wang, K. et al. Phase transition of NaGaO 2 at high pressure and high temperature. Solid State Commun. 152, 540–544 (2012). 126. Omata, T., Nagatani, H., Suzuki, I. & Kita, M. Wurtzite-derived ternary I-III-O2 semiconductors. Sci. Technol. Adv. Mater. 16, (2015). 127. Ash, J. T. & Grandinetti, P. J. Solid-state NMR characterization of 69Ga and 71Ga in crystalline solids. Magn. Reson. Chem. 44, 823–831 (2006). 128. Massiot, D. et al. 71Ga and 69Ga nuclear magnetic resonance study of B-Ga2O3: resolution of four- and six-fold coordinated Ga sites in static conditions. Solid State Nucl. Magn. Reson. 4, 241–248 (1995). 129. Božin, E. S. et al. Temperature dependent total scattering structural study of CaCu 3Ti4O12. J. Phys. Condens. Matter 16, (2004). 130. Tucker, M. C., Cheng, L. & Dejonghe, L. C. Selection of cathode contact materials for solid oxide fuel cells. J. Power Sources 196, 8313–8322 (2011). 131. López, M. L. et al. New dielectric anomalies in the A-site highly deficient NaxNbO3 electroceramics. Ceram. Int. 46, 16770–16780 (2020). 132. Vasylechko, L., Matkovski, A., Suchocki, A., Savytskii, D. & Syvorotka, I. Crystal structure of LaGaO3 and (La,Gd)GaO3 solid solutions. J. Alloys Compd. 286, 213–218 (1999). 133. Knight, K. S. Structural phase transitions, oxygen vacancy ordering and protonation in doped BaCeO3: Results from time-of-flight neutron powder diffraction investigations. Solid State Ionics 145, 275–294 (2001)."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier.grantnumber","label":"Dc Identifier Grantnumber","values":["2375383","ICASE"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/35611/1/Jordan%20Canton%20-%20Doping%20Mechanisms%20and%20Electrical%20Properties%20of%20Sodium%20Niobate.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Intermediate temperature solid oxide fuel cells (ITSOFCs) are one of many technologies attempting to decarbonise global energy production and utilise the hydrogen economy. Unfortunately, typical solid oxide electrolytes such as yttria-stabilised zirconia (YSZ) do not exhibit sufficient conductivity for operation in the intermediate temperature region (400-750 °C). As a result, many potential intermediate temperature solid oxide electrolytes have undergone investigation to replace YSZ. The goal of this project was to investigate the perovskite material NaNbO3 (NN) and identify its suitability as a solid oxide electrolyte. NN ceramics were prepared via solid-state reaction of mixed oxides at 900 °C, followed by sintering at temperatures in the range 1240-1350 °C. Physical properties of NN ceramics were assessed using X-Ray diffraction (XRD), Scanning Electron Microscopy (SEM), Electron Probe Micro Analysis (EPMA) and Nuclear Magnetic Resonance (NMR). Electrical properties were investigated using impedance spectroscopy to assess bulk conductivity and pO2 dependence of the ceramics, probostat measurements have allowed for determination of oxygen ion transport numbers (tion) and the electronic band gap of NN has been determined via UV-Vis spectroscopy. This project is divided into exploring the defect chemistry of NN and how it influences the electrical properties. It has been shown that NN produced via solid-state synthesis varies significantly compared to hydrothermally prepared, and commercially available NN powders. The variance has been attributed to non-stoichiometry between the sodium and niobium sites caused by sodium volatility during processing. Deliberate Na:Nb non-stoichiometry in the range 0.96-1.22 showcases that sodium rich NN exhibits greater bulk conductivities (55:45 NN σ500°C ≈ 26 μS cm-1) and promotes ionic conductivity, compared to sodium deficient NN (49:51 NN σ500°C ≈ 0.13 μS cm-1). The following doping mechanisms have been used to influence the electrical properties of NN: 1. Direct substitution of sodium for calcium to generate A-site vacancies: 2Na+ = Ca2+ 2. A-site donor doping using Mg2+ and Ga3+ for the reduction of oxygen vacancies: Na+ = Mg2+ + 0.5O2- 3. B-site donor doping using W6+ and Mo6+ for the reduction of oxygen vacancies: Nb5+ = W6+ + 0.5O2- 4. B-site acceptor doping using Mg2+, Ga3+ and Ti4+ for the generation of oxygen vacancies: Nb5+ + O2- = Ga3+ Generation of A-site vacancies via calcium doping leads to an increase in bulk conductivity (Na0.9Ca0.05NbO3 σ500°C ≈ 2.7 μS cm-1), with low levels of ionic conductivity attributed to sodium ion conduction. Donor doping of the A-site using Mg2+ or Ga3+ has no significant effect on the bulk conductivity (Na0.99Mg0.01NbO3.005 σ500°C ≈ 0.24 μS cm-1), however, ionic conductivity is supressed. Similarly, donor doping the B-site with W6+ supresses ionic conductivity without influencing bulk conductivity (NaNb0.99W0.01O3.005 σ500 °C ≈ 0.69 μS cm-1). However, doping with molybdenum does not appear to be successful due to preferential formation of a molybdenum bronze. Acceptor doping of the B-site with Ga3+ and Ti4+ promotes ionic conductivity and greatly enhances bulk conductivity (NaNb0.95Ga0.05O2.95 σ500 °C ≈ 0.08 mS cm-1/NaNb0.95Ti0.05O2.975 σ500 °C ≈ 0.05 mS cm-1). It has been shown that in gallium doped NN maximum conductivities are achieved at very low concentrations (<1at%) of dopant due to pinning of oxygen vacancies. Acceptor doping with Mg2+ appears to be unsuccessful due to a preference for A-site donor doping. The properties of NN vary significantly according to the dopant mechanism utilised, and the Na:Nb ratio. The electronic band gap of NN appears to be unaffected by acceptor doping and remains 3.4 eV. Oxygen ion transport numbers for acceptor doped NN ceramics indicate that all variants are mixed oxide ion-electronic conductors (tion=0.2-0.7), indicating that NN based materials are unsuitable for applications as solid oxide electrolytes."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Doping Mechanisms and Electrical Properties of Sodium Niobate"]}]}],"canonical_facts":{"dc:contributor.advisor":["Sinclair, Derek"],"dc:contributor.sponsor":["UKRI","Johnson Matthey"],"dc:creator":["Canton, Jordan"],"dc:date":["2024-03"],"dc:date.issued":["2024-03"],"dc:description.abstract":["Intermediate temperature solid oxide fuel cells (ITSOFCs) are one of many technologies attempting to decarbonise global energy production and utilise the hydrogen economy. Unfortunately, typical solid oxide electrolytes such as yttria-stabilised zirconia (YSZ) do not exhibit sufficient conductivity for operation in the intermediate temperature region (400-750 °C). As a result, many potential intermediate temperature solid oxide electrolytes have undergone investigation to replace YSZ. The goal of this project was to investigate the perovskite material NaNbO3 (NN) and identify its suitability as a solid oxide electrolyte. NN ceramics were prepared via solid-state reaction of mixed oxides at 900 °C, followed by sintering at temperatures in the range 1240-1350 °C. Physical properties of NN ceramics were assessed using X-Ray diffraction (XRD), Scanning Electron Microscopy (SEM), Electron Probe Micro Analysis (EPMA) and Nuclear Magnetic Resonance (NMR). Electrical properties were investigated using impedance spectroscopy to assess bulk conductivity and pO2 dependence of the ceramics, probostat measurements have allowed for determination of oxygen ion transport numbers (tion) and the electronic band gap of NN has been determined via UV-Vis spectroscopy. This project is divided into exploring the defect chemistry of NN and how it influences the electrical properties. It has been shown that NN produced via solid-state synthesis varies significantly compared to hydrothermally prepared, and commercially available NN powders. The variance has been attributed to non-stoichiometry between the sodium and niobium sites caused by sodium volatility during processing. Deliberate Na:Nb non-stoichiometry in the range 0.96-1.22 showcases that sodium rich NN exhibits greater bulk conductivities (55:45 NN σ500°C ≈ 26 μS cm-1) and promotes ionic conductivity, compared to sodium deficient NN (49:51 NN σ500°C ≈ 0.13 μS cm-1). The following doping mechanisms have been used to influence the electrical properties of NN: 1. Direct substitution of sodium for calcium to generate A-site vacancies: 2Na+ = Ca2+ 2. A-site donor doping using Mg2+ and Ga3+ for the reduction of oxygen vacancies: Na+ = Mg2+ + 0.5O2- 3. B-site donor doping using W6+ and Mo6+ for the reduction of oxygen vacancies: Nb5+ = W6+ + 0.5O2- 4. B-site acceptor doping using Mg2+, Ga3+ and Ti4+ for the generation of oxygen vacancies: Nb5+ + O2- = Ga3+ Generation of A-site vacancies via calcium doping leads to an increase in bulk conductivity (Na0.9Ca0.05NbO3 σ500°C ≈ 2.7 μS cm-1), with low levels of ionic conductivity attributed to sodium ion conduction. Donor doping of the A-site using Mg2+ or Ga3+ has no significant effect on the bulk conductivity (Na0.99Mg0.01NbO3.005 σ500°C ≈ 0.24 μS cm-1), however, ionic conductivity is supressed. Similarly, donor doping the B-site with W6+ supresses ionic conductivity without influencing bulk conductivity (NaNb0.99W0.01O3.005 σ500 °C ≈ 0.69 μS cm-1). However, doping with molybdenum does not appear to be successful due to preferential formation of a molybdenum bronze. Acceptor doping of the B-site with Ga3+ and Ti4+ promotes ionic conductivity and greatly enhances bulk conductivity (NaNb0.95Ga0.05O2.95 σ500 °C ≈ 0.08 mS cm-1/NaNb0.95Ti0.05O2.975 σ500 °C ≈ 0.05 mS cm-1). It has been shown that in gallium doped NN maximum conductivities are achieved at very low concentrations (<1at%) of dopant due to pinning of oxygen vacancies. Acceptor doping with Mg2+ appears to be unsuccessful due to a preference for A-site donor doping. The properties of NN vary significantly according to the dopant mechanism utilised, and the Na:Nb ratio. The electronic band gap of NN appears to be unaffected by acceptor doping and remains 3.4 eV. Oxygen ion transport numbers for acceptor doped NN ceramics indicate that all variants are mixed oxide ion-electronic conductors (tion=0.2-0.7), indicating that NN based materials are unsuitable for applications as solid oxide electrolytes."],"dc:format":["text"],"dc:identifier.grantnumber":["2375383","ICASE"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/35611/1/Jordan%20Canton%20-%20Doping%20Mechanisms%20and%20Electrical%20Properties%20of%20Sodium%20Niobate.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.department":["Faculty of Engineering (Sheffield)","Materials Science and Engineering (Sheffield)"],"dc:publisher.institution":["University of Sheffield"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/35611/"],"dc:relation.references":["1. Ritchie, H. & Roser, M. Fossil fuels. Our World Data (2017). 2. Maslin, M. Global warming: a very short introduction. (OUP Oxford, 2008). 3. Shafiee, S. & Topal, E. When will fossil fuel reserves be diminished? Energy Policy 37, 181–189 (2009). 4. Iwata, H. & Okada, K. Greenhouse gas emissions and the role of the Kyoto Protocol. Environ. Econ. Policy Stud. 16, 325–342 (2014). 5. Murdock, H. E. Renewables 2019 Global Status Report Collaborative. (2019). 6. Whittingham, M. S. History, evolution, and future status of energy storage. Proc. IEEE 100, 1518–1534 (2012). 7. Marbán, G. & Valdés-Solís, T. Towards the hydrogen economy? Int. J. Hydrogen Energy 32, 1625–1637 (2007). 8. Xu, J. & Froment, G. F. Methane steam reforming, methanation and water‐gas shift: I. Intrinsic kinetics. AIChE J. 35, 88–96 (1989). 9. Stojić, D. L., Marčeta, M. P., Sovilj, S. P. & Miljanić, Š. S. Hydrogen generation from water electrolysis - Possibilities of energy saving. J. Power Sources 118, 315–319 (2003). 10. Vaghari, H., Jafarizadeh-Malmiri, H., Berenjian, A. & Anarjan, N. Recent advances in application of chitosan in fuel cells. Sustain. Chem. Process. 1, 16 (2013). 11. Grove, W. R. XXIV. On voltaic series and the combination of gases by platinum . London, Edinburgh, Dublin Philos. Mag. J. Sci. 14, 127–130 (1839). 12. Grove, W. R. On a gaseous voltaic battery. J. Franklin Inst. 35, 277–280 (1843). 13. Sealy, C. The problem with platinum. Mater. Today 11, 65–68 (2008). 14. Aguiar, P., Adjiman, C. S. & Brandon, N. P. Anode-supported intermediate temperature direct internal reforming solid oxide fuel cell. I: Model-based steady-state performance. J. Power Sources 138, 120–136 (2004). 15. Pei, P., Korom, S. F., Ling, K. & Nasah, J. Cost comparison of syngas production from natural gas conversion and underground coal gasification. Mitig. Adapt. Strateg. Glob. Chang. 21, 629–643 (2016). 16. Pritchard, D. F. & Rattigan, W. M. Hazards of liquid hydrogen: Position paper. 42 (2010). 17. Aloui, T. & Halouani, K. Analytical modeling of polarizations in a solid oxide fuel cell using biomass syngas product as fuel. Appl. Therm. Eng. 27, 731–737 (2007). 18. Minh, N. Q. Ceramic fuel cells. J. Am. Ceram. Soc. 76, 563–588 (1993). 19. Yang, Z., Xia, G. G., Li, X. H. & Stevenson, J. W. (Mn,Co)3O4 spinel coatings on ferritic stainless steels for SOFC interconnect applications. Int. J. Hydrogen Energy 32, 3648–3654 (2007). 20. Zhu, T., Fowler, D. E., Poeppelmeier, K. R., Han, M. & Barnett, S. A. Hydrogen Oxidation Mechanisms on Perovskite Solid Oxide Fuel Cell Anodes. J. Electrochem. Soc. 163, F952–F961 (2016). 21. Hibino, T., Wang, S., Kakimoto, S. & Sano, M. One-chamber solid oxide fuel cell constructed from a YSZ electrolyte with a Ni anode and LSM cathode. Solid State Ionics 127, 89–98 (2000). 22. Benjamin, T. G., Camara, E. H. & Marianowski, L. G. Handbook of fuel cell performance. (1980). 23. Yokokawa, H., Sakai, N., Horita, T. & Yamaji, K. Recent developments in solid oxide fuel cell materials. Fuel cells 1, 117–131 (2001). 24. Yang, Z., Weil, K. S., Paxton, D. M. & Stevenson, J. W. Selection and Evaluation of Heat-Resistant Alloys for SOFC Interconnect Applications. J. Electrochem. Soc. 150, A1188 (2003). 25. Zouhri, K., Shinneeb, M., Chikhalsouk, M. & Cress, J. Solid oxide fuel cell cathode diffusion polarization: materials and exergy study. Energy Convers. Manag. 231, 113865 (2021). 26. Zouhri, K., Shinneeb, M., Chikhalsouk, M. & Cress, J. Solid oxide fuel cell cathode diffusion polarization: materials and exergy study. Energy Convers. Manag. 231, 113865 (2021). 27. Huang, K., Zampieri, A. & Ise, M. Cathode Polarizations of a Cathode-Supported Solid Oxide Fuel Cell. J. Electrochem. Soc. 157, B1471 (2010). 28. Takeguchi, T., Kikuchi, R., Yano, T., Eguchi, K. & Murata, K. Effect of precious metal addition to Ni-YSZ cermet on reforming of CH 4 and electrochemical activity as SOFC anode. Catal. Today 84, 217–222 (2003). 29. Tao, S. & Irvine, J. T. S. A redox-stable efficient anode for solid-oxide fuel cells. Nat. Mater. 2, 320–323 (2003). 30. Zhe, Y., Qizhao, L. & Zhu, B. Thermodynamic analysis of ITSOFC hybrid system for polygenerations. Int. J. Hydrogen Energy 35, 2824–2828 (2010). 31. Shen, J. P. & Song, C. Influence of preparation method on performance of Cu/Zn-based catalysts for low-temperature steam reforming and oxidative steam reforming of methanol for H2 production for fuel cells. Catal. Today 77, 89–98 (2002). 32. Basagiannis, A. C., Panagiotopoulou, P. & Verykios, X. E. Low temperature steam reforming of ethanol over supported noble metal catalysts. Top. Catal. 51, 2–12 (2008). 33. Vivanpatarakij, S., Aiouache, F. & Assabumrungrat, S. Performance of an improved combination unit of Pd-membrane methane steam reformer and intermediate temperature solid oxide fuel cell (C-Pd-ITSOFC). Int. J. Hydrogen Energy 40, 1894–1901 (2015). 34. Brett, D. J. L., Atkinson, A., Brandon, N. P. & Skinner, S. J. Intermediate temperature solid oxide fuel cells. Chem. Soc. Rev. 37, 1568–1578 (2008). 35. Kwon, O. H. & Choi, G. M. Electrical conductivity of thick film YSZ. Solid State Ionics 177, 3057–3062 (2006). 36. Sammes, N. M. & Zhihong, C. Ionic conductivity of ceria/yttria stabilized zirconia electrolyte materials. Solid State Ionics 100, 39–44 (1997). 37. Han, M., Tang, X., Yin, H. & Peng, S. Fabrication, microstructure and properties of a YSZ electrolyte for SOFCs. J. Power Sources 165, 757–763 (2007). 38. Jasinski, P., Petrovsky, V., Suzuki, T., Petrovsky, T. & Anderson, H. U. Electrical Properties of YSZ Films Prepared by Net Shape Technology. J. Electrochem. Soc. 152, A454 (2005). 39. Ishigaki, T., Yamauchi, S., Kishio, K., Mizusaki, J. & Fueki, K. Diffusion of oxide ion vacancies in perovskite-type oxides. J. Solid State Chem. 73, 179–187 (1988). 40. Esaka, T. Oxide Ion Conduction via Interstitial Sites in the Substituted Scheelite-and Spinel-type Oxides. Electrochemistry 78, 16–22 (2010). 41. Zhu, B. Functional ceria-salt-composite materials for advanced ITSOFC applications. J. Power Sources 114, 1–9 (2003). 42. Zhu, B., Fan, L. & Lund, P. Breakthrough fuel cell technology using ceria-based multi-functional nanocomposites. Appl. Energy 106, 163–175 (2013). 43. Gil, V., Moure, C. & Tartaj, J. Sinterability, microstructures and electrical properties of Ni/Gd-doped ceria cermets used as anode materials for SOFCs. J. Eur. Ceram. Soc. 27, 4205–4209 (2007). 44. Lacorre, P., Goutenoire, F., Bohnke, O., Retoux, R. & Laligant, Y. Designing fast oxide-ion conductors. Nature 404, 9–11 (2000). 45. Goutenoire, F., Isnard, O., Retoux, R. & Lacorre, P. Crystal structure of La2Mo2O9, a new fast oxide-ion conductor. Chem. Mater. 12, 2575–2580 (2000). 46. Georges, S. et al. The LAMOX Family of Fast Oxide-Ion Conductors: Overview and Recent Results. J. New Mater. Electrochem. Syst. 7, 51–57 (2004). 47. Evans, I. R., Howard, J. A. K. & Evans, J. S. O. The Crystal Structure of α-La2Mo2O9 and the Structural Origin of the Oxide Ion Migration Pathway. Chem. Mater. 17, 4074–4077 (2005). 48. Le, M. V., Tsai, D. S. & Nguyen, T. A. BSCF/GDC as a refined cathode to the single-chamber solid oxide fuel cell based on a LAMOX electrolyte. Ceram. Int. 44, 1726–1730 (2018). 49. Yokokawa, H. Understanding Materials Compatibility. Annu. Rev. Mater. Res. 33, 581–610 (2003). 50. Mitchell, R. H. Perovskites Modern and Ancient. (2002). 51. Megaw, H. D. Crystal structure of double oxides of the perovskite type. Proc. Phys. Soc. 58, 133–152 (1946). 52. Howard, C. J. & Stokes, H. T. Group-theoretical analysis of octahedral tilting in perovskites. Acta Crystallogr. Sect. B Struct. Sci. 54, 782–789 (1998). 53. Glazer, A. M. The classification of tilted octahedra in perovskites. Acta Crystallogr. Sect. B Struct. Crystallogr. Cryst. Chem. 28, 3384–3392 (1972). 54. Ishihara, T., Matsuda, H. & Takita, Y. Doped LaGaO3 Perovskite Type Oxide as a New Oxide Ionic Conductor. J. Am. Chem. Soc. 116, 3801–3803 (1994). 55. Huang, P. Superior Oxygen Ion Conductivity of Lanthanum Gallate Doped with Strontium and Magnesium. J. Electrochem. Soc. 143, 1644 (1996). 56. Huang, P., Horky, A. & Petric, A. Interfacial reaction between nickel oxide and lanthanum gallate during sintering and its effect on conductivity. J. Am. Ceram. Soc. 82, 2402–2406 (1999). 57. Fergus, J. W. Electrolytes for solid oxide fuel cells. J. Power Sources 162, 30–40 (2006). 58. Li, M. et al. A family of oxide ion conductors based on the ferroelectric perovskite Na0.5Bi0.5TiO3. Nat. Mater. 13, 31–35 (2014). 59. Yang, F. et al. Defect chemistry and electrical properties of sodium bismuth titanate perovskite. J. Mater. Chem. A 6, 5243–5254 (2018). 60. Lu, Y., López, C. A., Wang, J., Alonso, J. A. & Sun, C. Insight into the structure and functional application of Mg-doped Na0.5Bi0.5TiO3 electrolyte for solid oxide fuel cells. J. Alloys Compd. 752, 213–219 (2018). 61. Shafer, M. W. & Roy, R. Phase equilibria in the system Na2O–Nb2O5. J. Am. Ceram. Soc. 42, 482–486 (1959). 62. Egerton, L. & Dillon, D. M. Piezoelectric and dielectric properties of ceramics in the system potassium—sodium niobate. J. Am. Ceram. Soc. 42, 438–442 (1959). 63. Li, P. et al. Mechanism of significantly enhanced piezoelectric performance and stability in textured potassium-sodium niobate piezoelectric ceramics. J. Eur. Ceram. Soc. 38, 75–83 (2018). 64. Megaw, H. D. The Seven Phases of Sodium Niobate. Ferroelectrics 7, 87–89 (1974). 65. Cross, L. E. & Nicholson, B. J. LV. The optical and electrical properties of single crystals of sodium niobate. London, Edinburgh, Dublin Philos. Mag. J. Sci. 46, 453–466 (1955). 66. Reznichenko, L. A. et al. Structural instabilities, incommensurate modulations and P and Q phases in sodium niobate in the temperature range 300-500 K. Crystallogr. Reports 48, 448–456 (2003). 67. Wang, X. B. et al. High temperature Raman study of phase transitions in antiferroelectric NaNbO3. J. Mol. Struct. 385, 1–6 (1996). 68. Glazer, A. M. & Megaw, H. D. Studies of the lattice parameters and domains in the phase transitions of NaNbO3. Acta Crystallogr. Sect. A 29, 489–495 (1973). 69. Zhang, M. H., Fulanović, L., Zhao, C. & Koruza, J. Review on field-induced phase transitions in lead-free NaNbO3-based antiferroelectric perovskite oxides for energy storage. J. Mater. 9, 1–18 (2023). 70. Liu, W., Zhao, D. & Li, S. Large electrostrain with good temperature stability in sodium niobate based ceramics. RSC Adv. 7, 2550–2554 (2017). 71. Wu, J., Xiao, D. & Zhu, J. Potassium-sodium niobate lead-free piezoelectric materials: Past, present, and future of phase boundaries. Chem. Rev. 115, 2559–2595 (2015). 72. Zhang, H., Yang, B., Yan, H. & Abrahams, I. Isolation of a ferroelectric intermediate phase in antiferroelectric dense sodium niobate ceramics. Acta Mater. 179, 255–261 (2019). 73. Shao, T. et al. Potassium-sodium niobate based lead-free ceramics: novel electrical energy storage materials. J. Mater. Chem. A 5, 554–563 (2017). 74. Yang, Z. et al. Significantly enhanced recoverable energy storage density in potassium-sodium niobate-based lead free ceramics. J. Mater. Chem. A 4, 13778–13785 (2016). 75. Luo, N. et al. Well-defined double hysteresis loop in NaNbO3 antiferroelectrics. Nat. Commun. 14, 1776 (2023). 76. Zhang, M. H. et al. Electric-field-induced antiferroelectric to ferroelectric phase transition in polycrystalline NaNbO3. Acta Mater. 200, 127–135 (2020). 77. Tan, X., Ma, C., Frederick, J., Beckman, S. & Webber, K. G. The antiferroelectric ↔ ferroelectric phase transition in lead-containing and lead-free perovskite ceramics. J. Am. Ceram. Soc. 94, 4091–4107 (2011). 78. Zhang, M.-H. et al. Tailoring high-energy storage NaNbO3-based materials from antiferroelectric to relaxor states. Nat. Commun. 2023 141 14, 1–11 (2023). 79. Levin, I. et al. Displacive Order–Disorder Behavior and Intrinsic Clustering of Lattice Distortions in Bi-Substituted NaNbO3. Adv. Funct. Mater. 2001840, 1–13 (2020). 80. Lei, X. et al. Realizing oxygen ion conduction in perovskite structure NaNbO3 by A-site Bismuth doping. J. Alloys Compd. 924, 2–6 (2022). 81. Gouget, G. et al. High Ionic Conductivity in Oxygen-Deficient Ti-Substituted Sodium Niobates and the Key Role of Structural Features. Chem. Mater. 31, 2828–2841 (2019). 82. Gouget, G. et al. Associating and Tuning Sodium and Oxygen Mixed-Ion Conduction in Niobium-Based Perovskites. Adv. Funct. Mater. 30, 1–12 (2020). 83. Zhang, Z. T., Sridhar, S. & Cho, J. W. An investigation of the evaporation of B2O3 and Na2O in f-free mold slags. ISIJ Int. 51, 80–87 (2011). 84. Lee, Y. H., Cho, J. H., Kim, B. I. & Choi, D. K. Piezoelectric properties and densification based on control of volatile mass of potassium and sodium in (K0.5Na0.5)NbO3 ceramics. Jpn. J. Appl. Phys. 47, 4620–4622 (2008). 85. Shimizu, H., Kobayashi, K., Mizuno, Y. & Randall, C. A. Advantages of low partial pressure of oxygen processing of alkali niobate: NaNbO3. J. Am. Ceram. Soc. 97, 1791–1796 (2014). 86. Ferrarelli, M. C., Nuzhnyy, D., Sinclair, D. C. & Kamba, S. Soft-mode behavior and incipient ferroelectricity in Na1/2 Bi1/2 Cu3 Ti4 O12. Phys. Rev. B - Condens. Matter Mater. Phys. 81, 1–7 (2010). 87. Samara, G. A. The relaxational properties of compositionally disordered ABO3 perovskites. J. Phys. Condens. Matter 15, (2003). 88. Kamba, S. et al. Ferroelectric and incipient ferroelectric properties of a novel Sr 9-xPbxCe2Ti2O36(x = 0-9) ceramic system. Chem. Mater. 21, 811–819 (2009). 89. Tagantsev, A. K., Sherman, V. O., Astafiev, K. F., Venkatesh, J. & Setter, N. Ferroelectric materials for microwave tunable applications. J. electroceramics 11, 5–66 (2003). 90. Yadav, A., Pyare, R., Goodenough, J. B. & Singh, P. KTa1- x- yTixGeyO3-δ: A High κ Relaxor Dielectric and Superior Oxide-Ion Electrolyte for IT-SOFC. ACS Appl. Energy Mater. 3, 3205–3211 (2020). 91. Tsvetkov, D. S., Sereda, V. V., Malyshkin, D. A., Ivanov, I. L. & Zuev, A. Y. Chemical lattice strain in nonstoichiometric oxides: an overview. J. Mater. Chem. A 10, 6351–6375 (2022). 92. Gao, R. et al. Designing Optimal Perovskite Structure for High Ionic Conduction. Adv. Mater. 32, 1–9 (2020). 93. Fresno, F. et al. CO2 reduction over NaNbO3 and NaTaO3 perovskite photocatalysts. Photochem. Photobiol. Sci. 16, 17–23 (2017). 94. Handoko, A. D. & Goh, G. K. L. Hydrothermal synthesis of sodium potassium niobate solid solutions at 200 °C. Green Chem. 12, 680–68 (2010). 95. Van Hoek, C. & Koolwijk, M. Conventional wavelength dispersive spectroscopy versus parallel beam spectroscopy - A basic overview. Microchim. Acta 161, 287–293 (2008). 96. Makuła, P., Pacia, M. & Macyk, W. How To Correctly Determine the Band Gap Energy of Modified Semiconductor Photocatalysts Based on UV-Vis Spectra. J. Phys. Chem. Lett. 9, 6814–6817 (2018). 97. Jonscher, A. K. Dielectric relaxation in solids. J. Phys. D. Appl. Phys. 32, R57 (1999). 98. Sinclair, D. C. Characterization of Electro-materials using ac Impedance Spectroscopy. Bol. la Soc. Esp. Ceram. y Vidr. 65, 55–66 (1995). 99. Bruncková, H., Medvecký, L. & Hvizdoš, P. Effect of substrate on phase formation and surface morphology of sol-gel lead-free KNbO3, NaNbO3, and K0.5Na 0.5NbO3 thin films. Chem. Pap. 66, 748–756 (2012). 100. Lee, S., Liu, Z. K., Kim, M. H. & Randall, C. A. Influence of nonstoichiometry on ferroelectric phase transition in BaTiO3. J. Appl. Phys. 101, 1–8 (2007). 101. Ruf, T. et al. The influence on sintering and properties of sodium niobate (NaNbO 3 ) ceramics by “non-stoichiometric” precursor compositions. Mater. Chem. Phys. 229, 437–447 (2019). 102. Shakhovoy, R. A. et al. Ferroelectric Q and antiferroelectric P phases’ coexistence and local phase transitions in oxygen-deficient NaNbO3 single crystal: Micro-Raman, dielectric and dilatometric studies. J. Raman Spectrosc. 43, 1141–1145 (2012). 103. Irvine, J. T. S., Sinclair, D. C. & West, A. R. Electroceramics: Characterization by Impedance Spectroscopy. Adv. Mater. 2, 132–138 (1990). 104. Guo, H., Shimizu, H., Mizuno, Y. & Randall, C. A. Strategy for stabilization of the antiferroelectric phase (Pbma) over the metastable ferroelectric phase (P21ma) to establish double loop hysteresis in lead-free (1-x)NaNbO3-x SrZrO3 solid solution. J. Appl. Phys. 117, 214103 (2015). 105. Masó, N., Woodward, D. I., Várez, A. & West, A. R. Polymorphism, structural characterisation and electrical properties of Na2Nb4O11. J. Mater. Chem. 21, 12096–12102 (2011). 106. Romeu, M. C. et al. Impedance spectroscopy study of TiO2 addition on the ceramic matrix Na2Nb4O11. J. Mater. Sci. Mater. Electron. 24, 4993–4999 (2013). 107. Näfe, H., Amin, R. & Aldinger, F. Thermodynamic Characterization of the Eutectic Phase Mixture NaNbO3/Na3NbO4. II: Solid-State Electrochemical Investigation. J. Am. Ceram. Soc. 90, 3227–3232 (2007). 108. Liu, W. Dielectric and sintering properties of NaNbO3 ceramic prepared by Pechini method. J. Electroceramics 31, 376–381 (2013). 109. Lee, B.-K., Chung, S.-Y. & Kang, S.-J. L. Grain boundary faceting and abnormal grain growth in BaTiO3. Acta Mater. 48, 1575–1580 (2000). 110. Aso, S., Matsuo, H. & Noguchi, Y. Reversible electric-field-induced phase transition in Ca-modified NaNbO3 perovskites for energy storage applications. Sci. Rep. 13, 1–10 (2023). 111. Shannon, R. D. Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Crystallogr. Sect. A Cryst. physics, diffraction, Theor. Gen. Crystallogr. 32, 751–767 (1976). 112. Valant, M. et al. The origin of magnetism in Mn-doped SrTiO 3. Adv. Funct. Mater. 22, 2114–2122 (2012). 113. Choudhury, D. et al. Tuning of dielectric properties and magnetism of SrTiO3 by site-specific doping of Mn. Phys. Rev. B - Condens. Matter Mater. Phys. 84, (2011). 114. Tkach, A., Vilarinho, P. M. & Kholkin, A. L. Polar behavior in Mn-doped SrTiO3 ceramics. Appl. Phys. Lett. 86, 1–3 (2005). 115. Ren, P. et al. Mixed oxide ion and proton conduction and p-type semiconduction in BaTi0.98Ca0.02O2.98 ceramics. J. Mater. Chem. C 1, 2426–2432 (2013). 116. Shi, H., Lu, M., Lan, B. & Zhang, C. Effects of (Mo/W, N) codoping on electronic structures of NaNbO3 based on hybrid density functional calculations. Mod. Phys. Lett. B 32, 1–10 (2018). 117. Roth, R. S. & Waring, J. L. Phase equilibria as related to crystal structure in the system niobium pentoxide-tungsten trioxide. J. Res. Natl. Bur. Stand. Sect. A Phys. Chem. 70A, 281 (1966). 118. West, A. R. Basic Solid State Chemistry. (John Wiley & Sons, Ltd, 1999). 119. Dickens, P. G. & Whittingham, M. S. The tungsten bronzes and related compounds. Q. Rev. Chem. Soc. 22, 30–44 (1968). 120. Wold, A., Kunnmann, W., Arnott, R. J. & Ferretti, A. Preparation and Properties of Sodium and Potassium Molybdenum Bronze Crystals. Inorg. Chem. 3, 545–547 (1964). 121. Ananta, S., Brydson, R. & Thomas, N. W. Synthesis, formation and Characterisation of MgNb2O6 Powder in a Columbite-like Phase. J. Eur. Ceram. Soc. 19, 355–362 (1999). 122. Yang, F., Wu, P. & Sinclair, D. C. Electrical conductivity and conduction mechanisms in (Na0.5Bi0.5TiO3)1−x(BiScO3)x (0.00 ≤ x ≤ 0.25) solid solutions. J. Mater. Chem. C 6, 11598–11607 (2018). 123. Bottelberghs, P. H. & Everts, E. Charge carriers and dc polarization phenomena in solid Na2WO4. J. Solid State Chem. 14, 342–348 (1975). 124. Groszewicz, P. B. et al. The fate of aluminium in (Na,Bi)TiO3-based ionic conductors. J. Mater. Chem. A 8, 18188–18197 (2020). 125. Wang, K. et al. Phase transition of NaGaO 2 at high pressure and high temperature. Solid State Commun. 152, 540–544 (2012). 126. Omata, T., Nagatani, H., Suzuki, I. & Kita, M. Wurtzite-derived ternary I-III-O2 semiconductors. Sci. Technol. Adv. Mater. 16, (2015). 127. Ash, J. T. & Grandinetti, P. J. Solid-state NMR characterization of 69Ga and 71Ga in crystalline solids. Magn. Reson. Chem. 44, 823–831 (2006). 128. Massiot, D. et al. 71Ga and 69Ga nuclear magnetic resonance study of B-Ga2O3: resolution of four- and six-fold coordinated Ga sites in static conditions. Solid State Nucl. Magn. Reson. 4, 241–248 (1995). 129. Božin, E. S. et al. Temperature dependent total scattering structural study of CaCu 3Ti4O12. J. Phys. Condens. Matter 16, (2004). 130. Tucker, M. C., Cheng, L. & Dejonghe, L. C. Selection of cathode contact materials for solid oxide fuel cells. J. Power Sources 196, 8313–8322 (2011). 131. López, M. L. et al. New dielectric anomalies in the A-site highly deficient NaxNbO3 electroceramics. Ceram. Int. 46, 16770–16780 (2020). 132. Vasylechko, L., Matkovski, A., Suchocki, A., Savytskii, D. & Syvorotka, I. Crystal structure of LaGaO3 and (La,Gd)GaO3 solid solutions. J. Alloys Compd. 286, 213–218 (1999). 133. Knight, K. S. Structural phase transitions, oxygen vacancy ordering and protonation in doped BaCeO3: Results from time-of-flight neutron powder diffraction investigations. Solid State Ionics 145, 275–294 (2001)."],"dcterms:accessrights":["public"],"dc:title":["Doping Mechanisms and Electrical Properties of Sodium Niobate"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"],"person:identifier.orcid":["0009000590977513"]},"updated_at":"2026-11-18T23:27:55Z"}