{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:7320"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:7320","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Seawater as a hydraulic fluid; corrosion mechanisms and rates of engineering materials","abstract":"With the increasing demand for environmentally friendly hydraulic fluids in the oil and gas sector, recent advances in hydraulic technology have sparked renewed interest in the application of water instead of oil. For industry, using seawater as a hydraulic fluid would bring many benefits as it can be discharged to the sea. The main corrosion challenges associated with the use of seawater are addressed in this study, particularly on how to extend the material life when corrosion attack is likely to be very severe. On the other hand, the material’s degradation which is common in subsea applications is studied in detail which includes how corrosion mechanisms occur. The materials chosen in this research are those which are used extensively in subsea applications especially in Directional Control Valves (DCV) and piping operating with hydraulic fluids namely: (1) carbon steel, (2) stainless steel, and (3) cermet alloys (WC-Ni and WC-Co). As an active material, carbon steelcorrodes in a general way whereas passive materials such as stainless steel are more prone to localised corrosion which is often more catastrophic and difficult to predict and detect. However, cermets alloys (WC-Ni and WC-Co) which consist of metals and ceramics may exhibit both active and passive trends. Electrochemistry methods which are used in this study provide quantitative data which demonstrates different major corrosion parameters. Generally, temperature, oxygen, anions and pH are the main parameters that affect corrosion attack. In this research the effects of temperature, sulphate to chloride ratio and oxygen were studied on corrosion performance of DCV materials and compared the performance in seawater with a typical commercial hydraulic fluidHW443. From the analysis, it shows that temperature has a severe impact on corrosion rate, but alteration of sulphate to chloride ratio could decrease the corrosion rate close to HW443. Therefore, it is clear that by changing the sulphate/chloride ratio in seawater and adding green corrosion inhibitor similar performance to that compared to the use of commercial hydraulicfluids yet reduce the environmental harm on discharge could be attained. The thesis also presents information ofgeneric interest in corrosion of carbon steel and other materials of interest in subsea environments. Corrosion trends of carbon steel, stainless steel and WC-cermets and their prevalent corrosion mechanisms (from electrochemical analysis) are discussed.","abstract_html":"With the increasing demand for environmentally friendly hydraulic fluids in the oil and gas sector, recent advances in hydraulic technology have sparked renewed interest in the application of water instead of oil. For industry, using seawater as a hydraulic fluid would bring many benefits as it can be discharged to the sea. The main corrosion challenges associated with the use of seawater are addressed in this study, particularly on how to extend the material life when corrosion attack is likely to be very severe. On the other hand, the material’s degradation which is common in subsea applications is studied in detail which includes how corrosion mechanisms occur. The materials chosen in this research are those which are used extensively in subsea applications especially in Directional Control Valves (DCV) and piping operating with hydraulic fluids namely: (1) carbon steel, (2) stainless steel, and (3) cermet alloys (WC-Ni and WC-Co). As an active material, carbon steelcorrodes in a general way whereas passive materials such as stainless steel are more prone to localised corrosion which is often more catastrophic and difficult to predict and detect. However, cermets alloys (WC-Ni and WC-Co) which consist of metals and ceramics may exhibit both active and passive trends. Electrochemistry methods which are used in this study provide quantitative data which demonstrates different major corrosion parameters. Generally, temperature, oxygen, anions and pH are the main parameters that affect corrosion attack. In this research the effects of temperature, sulphate to chloride ratio and oxygen were studied on corrosion performance of DCV materials and compared the performance in seawater with a typical commercial hydraulic fluidHW443. From the analysis, it shows that temperature has a severe impact on corrosion rate, but alteration of sulphate to chloride ratio could decrease the corrosion rate close to HW443. Therefore, it is clear that by changing the sulphate/chloride ratio in seawater and adding green corrosion inhibitor similar performance to that compared to the use of commercial hydraulicfluids yet reduce the environmental harm on discharge could be attained. The thesis also presents information ofgeneric interest in corrosion of carbon steel and other materials of interest in subsea environments. Corrosion trends of carbon steel, stainless steel and WC-cermets and their prevalent corrosion mechanisms (from electrochemical analysis) are discussed.","abstract_has_math":false,"creators":["Ismail, Azzura"],"institution":"University of Leeds","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Neville, Anne"],"committee_chairs":[],"committee_members":[],"year":2014,"date_issued":"2014-01","date_published":"2014-01","updated_at":"2026-11-18T21:28:06Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.634276"],"render_values":[{"text":"uk.bl.ethos.634276","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/7320/1/Thesis%20final.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A7320","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Neville, Anne"]},{"key":"dc:contributor.sponsor","label":"Sponsor","values":["Ministry of Higher Education Malaysia","Aker Solutions, Aberdeen"]},{"key":"dc:creator","label":"Author","values":["Ismail, Azzura"]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2014-01"]},{"key":"dc:date.issued","label":"Date","values":["2014-01"]},{"key":"dc:publisher.commercial","label":"Dc Publisher Commercial","values":["University of Leeds"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["Institute of Engineering Thermofluids, Surfaces & Interfaces (iETSI) (Leeds)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Leeds"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/7320/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["1. Fontana M.G. Corrosion Engineering, McGraw-Hill, 1987, pp. 3-13. 2. Koch, G.H., Michiel P.H. and Thompson N.G.,Corrosion costs and preventive strategies in the United States,Federal Highway Administration (FHWA). FHWA-RD-01-156[online], 2001, [Accessed Jan 2011]. Available from: http://www.corrosioncost.com/summary.htm 3. GuoB., Chacko J.,Ghalambor A., Offshore pipelines. Gulf Professional Publishing[online],2005,p.302. [Accessed October 2008]. Available from: http://books.google.com.my/books/about/Offshore_Pipelines. 4. Chen, M.A.,Influence of hydrolysis time on the structure and corrosion protective performance of (3-mercaptopropyl)triethoxysilane film on copper.Corrosion Science. In Press,2001 5. Mary Tiemann the Specialist in Environmental Policy and Adam Vann, the Legislative Attorney, Hydraulic Fracturing and Safe Drinking Water Act Issues 2 Congressional Research Service, July 12, 201, p.1-42 6. Group, N.E.P.D., Sustainable Development of North America’s Oil and Natural Gas Ensuring Plentiful Energy and a Clean Environment, 2001, Department of Energy: United States of America. p. 3. 7. Azeri, Chirag and Gunashli, Subsea Water Injection Development, 2004, Environmental & Socio Economic Impact Assesment Phase 3 8. Daniel R.S and Newell K.D, Fracturing of Oil and Gas Wells in Kansas, December 2011,Kansas Geological Survey Hydraulic, pp.1-6 9. Knight G.C. 1977, Water hydraulics:Application of water-based fluids to hydraulic systems.Tribology International,10(2): pp. 105-108. 10. Rushau G..R.,Oil and gas exploration and production, 1997. 11. McManus., W.M. Canning Ltd, 1996, Presentations hydraulic fluids for Angola. 12. Zheng, L., Corrosion in hydraulic fluids for subsea applications, in School of Mechanical Engineering2009, University of Leeds: United Kingdom. p. 219. 13. Roberg P.R., Corrosion engineering: Principles and practice: McGraw-Hill, 2008, pp 5, 169-177. 14. KamachiI U. M., Corrosion Science and Technology:Mechanism, Mitigation and Monitoring 2009, Mumbai: narosa publishing house. 15. Denis B., Randy E., Andrew H., Donald H., Shreekant M., and Tony M., Corrosion in the oil industry,Schlumberger Oilfield review[online], 1994, [Accessed 2010]. pp. 1-15.Available from:http://www.slb.com/~/media/Files/resources/oilfield_review/ors94/0494/p04_18.pdf 16. Butler G., H.C.K.I., Corrosion and Its Prevention in Waters1966: A Leonard Hill Book. 281. 17. ToolBox, T.E. Oxygen solubility in fresh and sea water. 2011; Available from: http://www.engineeringtoolbox.com/oxygen-solubility-water-d_841.html. 18. Stansbury E.E. and Buchanan R.A.,Fundamental of electrochemical corrosion, The University of Tennessee, ASM International, 2000. pp 172-197. 19. Shinagawa K, Anti-corrosion Measures for Cable Bearers and Other Iron Fittings in Manholes. NTT Technical Review [online], 2008. 6(11). [Assessed April 2011]. Available from: https://www.ntt-review.jp/archive. 20. Davis J.R., Corrosion:understanding the basics, Ohio, ASM International, 2000, pp 21. Dawson J.L., Corrosion monitoring of steel in concrete in crane. A.P. (ed) corrosion of reinforcement in concrete construction, 1983: p. 175-92. 22. Ahmad Z., Principles of Corrosion Engineering and Corrosion Control. 2006: p. 90-109. 23. Tait W.S., An introduction to electrochemistry corrosion testing for practicing engineers and scientist, 1994, PairODocs Publications. p. 119. 24. Revie R.W., Uhlig's Corrosion Handbook. John Wiley & Sons, 2nd ed, 2000 25. LiI J. et al., Critical pitting and repassivation temperatures for duplex stainless steel in chloride solutions. Electrochimica Acta, 2008. 53(16): p. 5220-5225. 26. Roberge P.R. Handbook of Corrosion Engineering, United States, McGraw Hill, 2008, 27. MalikA.U., Ahmad S., Andijani I.,Corrosion behavior of steels in Gulf seawater environment., Saline Water Conversion Corporation, [online], 1999. 123: pp. 205-213.[Accessed March 2011]. Availabe from : http://www.swcc.gov 28. Roberge P.R. [online]. 2000. [Accessed 19 May 2011]. Availabe from : http://www.corrosion-doctors.org/Forms-crevice/crevice1.htm. 29. FrankelG.S., Sridhar N., Understanding localized corrosion.[online], Materials Today, 2008. 11(10): p. 38-44. [Accessed 2011]. Available from: http://www.matsceng.ohio-state.edu/~frankel/fcc/pubs/data/102.pdf 30. Leckie H.P., UhligH.H., Environmental factor affecting the critical potential for pitting in 18-8 stainless steel.J.Electrochemical Society, 1966. 113(12): p. 1262-1267. 31. Galvele J.R., Transport processes in passivity breakdown-II. Full hydrolysis of the metal ions. Corrosion Science, 1981. 21(8): p. 551-579. 32. Schwenk W, Electrochemical investigations of pitting corrosion.Corrosion Science, 1973. 13(10): pp. 739-746. 33. Sastri V.S, Edward G. and Mimoun E.,Corrosion: Prevention and protection. Practical solutions2007: John Wiley & Sons, Ltd. 34. Watkins J.W. and Kincheloe W., Corrosion of steel in water by varied ratios of dissolved gasses. Corrosion, 1958. 14: p. 341-344. 35. Sridhar N., Brossia C.S, Dunn D.S. and Anderko A., Predicting localized corrosion in seawater. Corrosion, 2004. 60(10): p. 915-936. 36. Uhlig H. H. ,Triadis D.N., and Stern M., Effect of oxygen, chlorides and calcium ion on corrosion inhibition of iron by polyphosphates. J.Electrochemical Society, 1955. 102(2): p. 59-66. 37. CacerasL., Vargas T. and Parra M., Study of the variatonal patterns for corrosion kinetics of carbon steel as a function of dissolved oxygen and NaCl concentration. Electrchimica Acta, 2009. 54: p. 7435-7443. 38. Allen J.B., and Larry R.F., Electrochemical methods, Fundamentals and applications. 2nd ed2001: John WIley & Sons, Inc. 39. Hochstrasser(-Kurz) S.,Mueller Y.,Latkoczy C. and Virtanen S..,Analytical characterization of the corrosion mechanisms of WC–Co by electrochemical methods and inductively coupled plasma mass spectroscopy Corrosion Science, 2007. 49(4): p. 2002-2020. 40. Krkwood D., Microbial corrsion of metals in seawater. proceeding of a meeting organised by the Scottish Marine Biological Association, 1982: p. 16-19. 41. Grobe H. and Majewsky S.,Proportion of salt to sea water and chemical composition of sea salt, Institute for Polar and Marine Research, Bremerhaven, Germany[online], 2008. [Assessed 2009]. Available from: https://wwwalfred Wegener. 42. Mauchline J., Fouling and corrosion of metals in seawater. Science direct, 1982. : p. 281-292. 43. Todd B.,Materials Selection for High Reliability Seawater Systems,Nickel Development Institute[online], 2007. [Assessed 2008]. Available from: http://www.copper.org/applications/cuni/txt_materials_selection.html 44. BrownE., Seawaetr:its composition, properties and behaviour.England, Butterworth Heinemann in association with The Open University, 1999. 2: p. 14-17. 45. Takasaki S. and Yamada.Y., Effects of temperature and aggressive anions on corrosion of carbon steel in potable water. Corrosion Science, 2007. 49(1): p. 240-247. 46. Duthil, J.P., Mankowski, G. and Giusti A.,The synergetic effect of chloride and sulphate on pitting corrosion of copper. Corrosion Science, 1996. 38(10): p. 1839-1849. 47. Abd El Wanees,Abd El Haleem, S.M.,S., Abd El Aal, E.E. and Diab, E., Environmental factors affecting the corrosion behavior of reinforcing steel. IV. Variation in the pitting corrosion current in relation to the concentration of the aggressive and the inhibitive anions,Corrosion Science, 2010. 52(5): pp. 1675-1683. 48. Strehblow H.H. andTitze B., Pitting potentials and inhibition potentials of iron and nickel for different aggressive and inhibiting anions.Corrosion Science, 1977. 17(6). 49. El-Naggar M.M., Effects of Cl−, NO3− and SO42− anions on the anodic behavior of carbon steel in deaerated 0.50 M NaHCO3 solutions,Applied Surface Science, 2006. 252(18). 50. The Hendrix Group Reporter,Hydrogen Embrittlement of High Strength Fasteners![online].1997.7(1), [Accessed 2011], Available from:http://hghouston.com/resources/technical-newsletters/he-of-high-strength-fasteners.aspx 51. Lim, G.H., Chua P.S.K., and He Y.B., Modern water hydraulics--the new energy-transmission technology in fluid power,Applied Energy. 76(1-3): pp. 239-246. 52. Foszcz and Joseph L., \"Hydraulic fluid choices.\" Plant Engineering, 1996. 50(4): p. 68-72. 53. Agency, U.S.E.P., Exemption of oil and gas exploration and production wastes from federal hazardous waste regulations. 53. Knight G.C., Water Hydraulics. Application of water-based fluids to hydraulic systems, Tribology International, April 1977:pp. 105-107. 54. Naylor J. and McManus S., Hydraulic fluids and their future in a more environemntally conscious industry, Martson Bentley report, :. p.1-9 55. Zelman et al., Pipeline and Gas Technology [magazine],November/December 2008, Hart Energy Publishing, LP, p.50 56. Anon, The Centre for Environment, Fisheries & Aquaculture Science (Cefas),[online], 2008, [Assessed June 2011], Available from: http://www.cefas.co.uk/about-us.aspx. 57. Ernest W. K., Use of Corrosion Inhibitors on the Trans Alaska Pipeline, VCI Corrosion ControlSupplement to Materials Performance, January 2001 ORTEC CORP, pp 1-3 58. Ramesh S. and Rajeswari S.,Evaluation of inhibitors and biocide on the corrosion control of copper in neutral aqueous environment. Corrosion Science, 2005. 47(1): pp. 151-169. 59. AlentejanoC.R. and Aoki I.V, Localized corrosion inhibition of 304 stainless steel in pure water by oxyanions tungstate and molybdate. Electrochimica Acta, 2004. 49(17-18): p. 2779-2785. 60. Uhlig H.H., Structure and growth of thin films on metals exposed to oxygen Corrosion Science, 1967. 7(6): pp. 325-339. 61. Gregory R. R and Mohammed A. Al-Anezi., Oil and gas exploration and production. 2000. 62. Dudukcu M., Yazici B. and Erbil M., The effect of indole on the corrosion behaviour of stainless steel. Materials Chemistry and Physics, 2004. 87(1): p. 138-141. 63. Arshadi M.R., Parsafar Gh.A. and Sastri V.S., Cluster/polarized continuum models for density functional theory investigations of benzimidazole corrosion inhibitors at metal/solution interface. NACE International, 2006. 62(3): p. 199-206. 64 DelgadoA. V.,Gonzalez-Caballero F., R., Hunter J., Koopal L.K. and. Yklema J., Measurement and Interpretation of Electrokinetic Phenomena, International Union of Pure and Applied Chemistry Physical Biophysical Chemistry Division, 2005 77(10), pp. 1753–1805 65. Osman M.M., Corrosion inhibition of aluminium-brass in 3.5% NaCl solution and sea water. Materials Chemistry and Physics, 2001. 71(1): pp. 12-16. 66. Hosseini S.M.A., Salari M. and Motlagh M.G,Thioamide compounds as corrosion inhibitors for stainless steel in H2SO4 solution. NACE International, 2010. 66(11): pp. 115003:1-115003:12. 67. YurtA.,Balaban A., Kandemir S.U., Bereket G. and Erk B., Investigation on some Schiff bases as HCl corrosion inhibitors for carbon steel. Materials Chemistry and Physics, 2004. 85(2-3): pp. 420-426. 68. OmanovicS. and Ggreba S, Interaction of 12-aminododecanoic acid with a carbon steel surface:Towards the development of 'green' corrosion inhibitors. Corrosion Science, 2010. 52(6): p. 2104-2113. 69. Sethuraman M.G and.Kamal C., Spirulina platensis-A novel green inhibitor for acud corrosion of mild steel. Arabian Journal of Chemistry, 2010: pp. 1-7. 70. Khaled K.F., Experimental and theoretical study for corrosion inhibitor of mild steel in hydrochloric acid solution by some new hydrazine carbodithioic acid derivatives. Applied Surface Science, 2006. 252(12): p. 4120-4128. 71. Hosseini M.G., Ehteshamzadeh M. and Shahrabi T., Protection of mild steel corrosion with Schiff bases in 0.5 M H2SO4 solution. Electrchimica Acta, 2007. 52(11): p. 3680-3685. 72. LalithaA., Ramesh S. and Rajeswari S., Surface protection of copper in acid medium by azoles and surfactants. Electrchimica Acta, 2005. 51(1): p. 47-55. 73. Saracoglu, M., Zor S., KandemirliF. and ArslanT., Inhibition effects of amides on the corrosion of copper in 1.0 M HCl : Theoretical and experimental studies. NACE International, 2011. 67(12): p. 125003:1-11. 74. Myles M., Jordan N.F., David C.J., Morag and Morag E., Biodegradable scale inhibitors. Laboratory and filed evaluation of \"Green\" carbonate and sulpahte scale inhibitors with deployment histories in the north sea. Chemistry in the oil industry X. Oilfield Chemistry: REACHing the Solution, 2007. 1: pp. 286-308. 75. Division, P.A., The Harmonised Offshore Chemical Notifications Format (HOCNF) Scheme 2006. 76. Wm Canning Ltd, Marston Bentley Division, Cale Lane, Wigan, UK, Technical Manual: OCEANIC HW 600 series: Oceanic HW625, HW 640, HW660: Water based production control fluids for operation of high temperature, high pressure conventional oil and gas wells, 1998,:. 1-58. 77. Manganon P.L., The Principles of Materials Selection for Eingineering Design, Prentice Hall, 1999, pp.512-535. 78. Ueda M., Development of corrosion resistance alloys for the oil and gas industry-based on spontaneous passivity mechanism. NACE International, Corrosion conference, 2006. 62 (10): pp. 856-867. 79. Yang S., Guo J., Shang C. Wang Y. and He X.,Influence of carbon content and microstructure on corrosion behaviour of low alloy steels in a Cl- containing environment, Corrosion Science, 2008. 51 : pp. 242-251. 80. Xu J., Bright M. A., Liu X. and Barbero E., Liquid metal corrosion of 316L stainless steel, 410 stainless steel and 1015 carbon steel in a molten zinc bath, Metallurgical and Materials Transactions A, 2007. 38A: pp.2727-2736. 81. Andijani I. and Turgoose S., Studies on corrosion of carbon steel in deaerated saline solutions in presence of scle inhibitor, Gulf Conference, 1999.: pp. 2231-2246. 82. Lee J. S., Ray R.I., Lemieux E.J., Falster A. U., and Little B. J., An evaluation of carbon steel corrosion under stagnant seawater conditions, Biofouling, 2004. 20 (4/5):. pp. 237-247. 83. Nesmeyanoka, K.A., Effect of oxygen on steel corrosion in steam-water flows at a temperature of 280ºC, Atomnaya Energiya, 1969. 29 (2) :. pp. 781-785. 84. KamachiU.M., and Pujar M.G., Pitting Corrosion of Austenitic Stainless Steels and Their Wekdment. 2002, Narosa Publishing House, pp. 89-91. 85. Smith W.F., Principles of materials science and engineering1996: McGraw Hill. 86. Strafford K.N., Venkatesan K., Subramaniam C. and Green L.K.,Influence of chromium content on corrosion of plasma-nitrided steel, NACE International. 1997,53 (7) :. pp. 507-515. 87. NascimentoD., Ierardi M.C.F, Kina A.Y. and Tavares S.S.M.,Pitting corrosion resistance of cast duplex stainless steels in 3.5%NaCl solution. Materials Characterization, 2008. In Press, Corrected Proof: pp. 1-5. 88. MarcusP., Maurice V.and Strehblow H.H., Localised corrosion (pitting): A modelof passivity breakdown including the role of oxide layer nanostructure. Corrosion Science. 2008, 50:. pp. 2698-2704. 89. Cunha Belo M.D., Rondot B.,Compere C., Montemor M.F., Simões A.M.P., Ferreira M.G.S.,Chemical composition and semiconducting behaviour of stainless steel passive films in contact with artificial seawater. Corrosion Science, 1998. 40(2-3): pp. 481-494. 90. QvarfortR. and Olsson J., Transpassive corrosion of high alloy stainless steels and bickel base alloys, NACE International. 2002. 02133:.pp. 1-17. 91. Fredriksson W., Malmgren S., Gustafsson T., Gorgoi M. and Edstroma K.,Full depth proﬁle of passive ﬁlms on 316L stainless steel based on high resolution HAXPES in combination with ARXPS, Applied Surface Science, 2012. 258:. pp.5790–5797. 92. SouzaE.C., Sergio M., Rossiti and Rollo J.M.D.A Influence of chloride ion concentration and temperature on the electrochemical properties of passive films formed on a superduplex stainless steel. Science Direct, 2010:.pp.240-244. 93. Magellan Metals, Inconel 625[online]. 2004. [Accessed 7 April 2011], Available from: http://www.magellanmetals.com/inconel_625.html?gclid=CNi1v7LJiqgCFUdP4QodrXs6Cw. 94. Cunha Belo D., Hakiki M., Ferreira N.E., Belo M.G.S.,M. C. D and N.E. Hakiki, Semiconducting properties of passive films formed on nickel-base alloys type Alloy 600: infuence of the alloying elements.Electrochimica Acta , 1999, 44 :. pp.2473-2481. 95. WuX. , Huang J. and Han E.H.,,Influence of pH on electrochemical properties of passive films formed on Alloy 690 in high temperature aqueous environments. Corrosion Science, 2009 (51):. pp. 2976-2982. 96. Kawashima A., Asami K. and Hashimoto K.,An XPS study of passive films on nickel and alloy 600 in acids. Corrosion Science. 1985, 25(12):.pp.1103-1114. 97. Yin Z.F., Zhao W.Z., LaiW.Y.and Zhao X.H., Electrochemical behaviour of Ni-base alloys exposed under oi/gas field environments, Corrosion Science. 2009, 51 :.p. 1702-1706 98. Chen C. F., Jiang J., ZhengS.Q.,and Cui L.S.,The non-linear fitting method to study the semiconductor properties of passive films of Inconel alloy G, Journal of Electroanalytical Chemistry, 2011,658 :. p.52–56. 99. Marcus, P., Machet A., Galtayries A., Zanna S., Klein L., Maurice V., Jolivet P, M. Foucault P., Combrade and Scott P.,XPS and STM study of the growth and structure of passive films in high temperature water on a nickel-base alloy, Electrochimica Acta 2004.49 (4):. pp. 3957–3964. 100. YihS.W.H and Wang C.T., Tungsten: sources, metallurgy, properties, and applications1979: Plenum press, New York and London. 358-359. 101. Lekatou A., Zois D., Karantzalis A.E., and Griminelis D., Electrochemical behaviour of cermet coatings with a bond coat on A17075: Psedopassivatity, localized corrosion and galvanic effect considerations in a saline environment, Corrosion Science, 2010, 52, pp. 2616-2635. 102. ViljusM., Klaasena H., Kubarseppa J., Roosaara T., and Traksmaa R., Adhesive wear performance of hardmetals and cermets, Wear, 2010. 268: p. 1122-1128. 103. LacknerA. and Filzwieser A., Gas carburizing of tungsten carbide (WC) powder. U.S Patent 6447742, 2002. 104. Wells, Alexander F., Structural inorganic chemistry. 5 1945: Clarendon Press. p. 590. 105. Scholl H., Hofman B. and Rauscher A., Anodic polarization of cemented carbides of the type [(WC,M): M = Fe, Ni or Co] in sulphuric acid solution..Electrochimica Acta, 1992. 37(3): pp. 447-452. 106. Batchelor A.W., Loh .N.L. and Chandrasekaran M., Materials: Degradation and its control by surface engineering, 2002(2), Singapore: Imperial College Press. p. 412. 107. Upadhayaya G.S., Cemented Tungsten Carbides: Production, Properties, and Testing1998: Noyes Publications. p.403. 108. PotgieterJ.H., Thanjekwayo N., Olubambi P., Maledi N. and Potgieter-Vermaak S.S., Influence of Ru additions on the corrosion behaviour of WC-Co cemented carbide alloys in sufuric acid. Int. Journal of Refractory Metals and Hard Materials, 2011. 29:. pp. 478-487. 109. Buss K. Thesis: High temperature deformation mechanisms of cemented carbides and cermets. Institute of Complex Matter. France, 2004, p 8. 110. TomlinsonW.J. and Linzell C.R.,Anodic polarization and corrosion of cemented carbides with cobalt and nickel binders. Journal of Materials Science, 1988. 23(3): p. 914-918. 111. HumanA.M., Roebuch B. and ExnerH.E., Electrochemical polarization and corrosion behaviour of cobalt and Co (W,C) alloys in 1 N sulphuric acid.. Materials Science and Engineering , 1998. 241: p. 202-210. 112. Anik M.,Effect of concentration gradient on the anodic behavior of tungsten, Science Direct. 2006. 48, pp. 4158-4173. 113. Suleiman A., Skeldon P., Thompson G.E., Echeverria F., Graham M.J., Sproule G.I., Moisa S.,Quance T. and Habazaki H., Anodic oxides on InAlP formed in sodium tungstate electrolyte, Corrosion Science. 2010, 52, pp. 595-601. 114. Lekatou A., Regoutas E., Karantzalis A.E., Corrosion behaviour of cermet-based coatings with a bond coat in 0.5 M H2SO4, Corrosion Science. 2008. 50, pp. 3389-3400. 115. GhandehariM.H. ,Andersen T.N. and Eyring H., The electrochemical reduction of oxygen on copper in dilute sulphuric acid solutions. Corrosion Science, 1976. 16(3): p. 123-135. 116. Sutthiruangwong S. and Mori G., Corrosion properties of Co-based cemented carbides in acidic solutions. International Journals of Refractory Metals & Hard Materials, 2003. 21. pp. 135-145. 117. Warren A., Nylund A and Olefjord I., Oxidation of tungsten and tungsten carbide in dry and humid atmospheres. International Journals of Refractory Metals & Hard Materials, 1996. 14. pp. 345-353 118. Andersson K.M. and Bergstrom L., Oxidation and dissolution of tungsten carbide powder in water,International Journals of Refractory Metals & Hard Materials, 2000. 18. pp. 121-129. 119. Trueman A.R., Schweinsberg D.P. and Hope G.A., A study of the effect of cobalt additions on the corrosion of tungsten carbide/carbon steel metal matrix composites, Corrosion Science, 1999, 41, pp. 1377-1389. 120. Trueman A.R., Schweinsberg D.P., and Hope G.A., The effect of choromium additions on the corrosion behaviour of tungsten carbide/carbon steel metal matrix composites, Corrosion Science, 1998, 40 (10), pp. 1685-1696. 121. KirkovP., The influence of halide ion concentration on the effects of surface active inhibitors in strong electrolytes. Corrosion Science, 1973. 13(10): p. 697-706. 122. Pohjanne P., Carpen L., Kinnunen P., Ramo J., Sarpola A., Riihimaki M., and Hakkarainen T., Stainless steel pitting in chloride-sulfate solutions-the role of cations, 2007, NACE International, Corrosion conference and expo: USA. 123. Pyun P.I, Moon S., Ahn S.H. and Kim S.S.,Effects of Cl-, NO3- and SO42- ions on anodic dissolution of pure aluminium in alkaline solution. Corrosion Science, 1999. 41(4): p. 653-667. 124. Smialowska Z., Effect of the ratio of Cl-/SO42- in solution on the pitting corrosion of Ni. Corrosion Science, 1971. 11(4): p. 209-221. 125. Dechema Handbook of Corrosion, 11 ,Weinheim, NY:VCH Publishers, 1992:. p.66. 126. Hinds G., The electrochemistry of corrosion,[online]. 2006. [Accessed 2012], Available from: http://www.npl.co.uk/upload/pdf/the_electrochemistry 127. Melcher R.E., Effect on marine immersion corrosion of carbon content of low alloy steels. Science direct, 2003. 45(11): p. 2609-2625. 128 Adhikari A.V. and Saliyan V.R.,Quinoline-5-ylmethylene-3-{[8-(trifluromethyl)quinolin-4-yl]thio} propanohydrazide as an effecive inhibitor of mild steel corrosion in HCl solution.. Science direct, 2008. 50. pp.55-61. 129. Christov M. and Popova A., Adsorption characteristics of corrosion inhibitors from corrosion rate measurements.Corrosion Science, 2004. 46. pp.1613-1620. 130. Szklarska-Smialowska Z., The kinetics of pit growth on Ni in solutions with different Cl-/SO42- ratios. Corrosion Science, 1972. 12(6): pp. 527-536. 131. ThompsonN. G. and Payer J.H., DC electrochemical test methods. Vol. 6. 1998. 98. 132. Sedriks A.J., Corrosion stainless steel1979: John Wiley & Sons, New York. 282. 133. Scully J.C., The fundamentals of corrosion1966: Pergamon press. 192. 134. Ziemniak S.E. and Hanson M., Corrosion behavior of 304 stainless steel in high temperature, hydrogenated water. Corrosion Science, 2002. 44(10): p. 2209-2230. 135. Oguzie E.E., Corrosion inhibition of aluminium in acidic and alkaline media by Sansevieria trifasciata extract. Corrosion Science, 2007. 49(3): p. 1527-1539. 136. Stellwag B., The mechanism of oxide film formation on austenitic stainless steels in high temperature water. Corrosion Science, 1998. 40(2/3): p. 337-370. 137. Garfias-Mesias L. F., Sykes J.M.., Metastable pitting in 25 Cr duplex stainless steel. Corrosion Science, 1999. 41(5): p. 959-987. 138. Fischer K. P., SteenslandO., Steinsmo U. and Wallen,B., Comparison of seawater corrosivity in Europe, in EFC1996: UK. 139. Bardal E., Drugli J.M. and Gartland P. O., The behaviour of corrosion-resistant steels in seawater: A review Corrosion Science, 1993. 35(1-4): p. 257-267. 140. Dexter S. C. and Gao G.Y., Corrosion, 1988. 44: p. 717. 141. Laitinen T., Localized corrosion of stainless steel in chloride, sulfate and thiosulfate containing environments. Corrosion Science, 2000. 42(3): p. 421-441. 142. PistoriusP.C. and Burstein G.T., Growth of corrosion pits on stainless steel in chloride solution containing dilute sulphate. Corrosion science, 1992. 33(12): p. 1885-1897. 143. Engqvist H., Beste U. and Axén, N.,International Journal of Refractory Metals and Hard Materials. 2000. 18, 103-109. 144. Hochstrasser(-Kurz) S.,Mueller Y., Latkoczy C.,Virtanen S. and Schmutz P., Analytical characterization of the corrosion mechanisms of WC-Co by electrochemical methods and inductively coupled plasma mass spectrocopy. Corrosion Science, 2007. 49(4): p. 2002-2020. 145. Benedetto, B.,Fanigliulo A. and Mele C., Electrochemical oxidation of WC in acidic sulphate solution Corrosion Science, 2004. 46(2): p. 453-469. 146. Rosales, B.M.Vera, R., and Tapia, C.,Effect of the exposure angle in the corrosion rate of plain carbon steel in a marine atmosphere Corrosion Science, 2003. 45(2): p. 321-337. 147. Zhu, X., Lei, T., Characteristics and formation of corrosion product films of 70Cu-30Ni alloy in seawater. Corrosion Science, 2002. 44(1): p. 67-79. 148. Cáceres, L.,Vargas, T. and Herrera, L.,Determination of electrochemical parameters and corrosion rate for carbon steel in un-buffered sodium chloride solutions using a superposition model. Corrosion Science, 2007. 49(8): p. 3168-3184. 149. Larson, D.T., Surface analytic techniques in corrosion science. Corrosion Science, 1979. 19(10): p. 657-673. 150. Wren,Yazdanfar, K., Zhang, X., Keech, P.G,Shoesmith, D.W.,,Film conversion and breakdown process on carbon steel in the presence of halides. Corrosion Science, 2010. 52(4): p. 1297-1304. 151. Yang, G., Ying, L.,and Haichao, L.,Experimental studies on the local corrosion of low alloy steels in 3.5% NaCl. Corrosion Science, 2001. 43(3): p. 397-411. 152. Jordan, K.G., and Williams V.T., Popeye project: Hydraulic Umbilical, in Offshore Technology Conference, S.O.P. Company, Editor 1996, OTC: Texas. p. 113-120. 153. Melchers, R.E., and Jeffrey, R.,Early corrosion of mild steel in seawater, Corrosion Science, 2005, 47, pp. 1678-1693. 154. Machio, C.N., D.S.KONADU., J. van der Merwe, J.H. Potgieter, S. Potgieter-Vermaak, The corrosion behaviour of WC-VC-Co hardmetals in acidic media. Corrosion Science, 2010. 52(9): pp. 3118-3125. 155. N.J. Laycock, S.E.W., C.A. Johnson, P.T. Wilson, B.J. Webster, Pitting of Type 304 stainless steee in the presence of a biofilm containing sulphate reducing bacteria. Corrosion Science, 1998. 40(2-3): p. 465-480. 156. El-Sayed, A.-R., H.S. Mohran, and H.M. Abd El-Lateef, Potentiodynamic studies on anodic dissolution and passivation of tin, indium and tin-indium alloys in some fruit acids solutions. Corrosion Science, 2009. 51(11): p. 2675-2684. 157. J. Mankowski and Z.Szklarska-Smialowska., Studies on accumulation of chloride ions in pits growing during anodic polarization. Corrosion Science, 1975. 15(6-12): p. 493-501. 158. Jingyi, Z.P.M., Chunchun Xu Youping Liu, Kinetic and thermodynamic behaviour inside occluded corrosion cells interpreted by potential/pH diagrams Corrosion Science, 1989. 29(5): p. 557-566. 159. J.Mankowski, Z.S.-S., Studies on accumulation of chloride ions in pits growing during anodic polarization. Corrosion Science, 1975. 15(6-12): p. 493-501. 160. Wagner, C., Passivity and inhibition during the oxidation of metals at elevated temperatures. Corrosion Science, 1965. 5(11): p. 751-764. 161. Z.F. Yin, W.Z.Z., W.Y. Lai, X.H. Zhao, Electrochemical behaviour of Ni-base alloys exposed under oil/gas field environments. Corrosion Science, 2009. 51(8): p. 1702-1706. 162. Corvo, F., et al., Indoor atmospheric corrosion in Cuba. A report about indoor localized corrosion. Corrosion Science, 2007. 49(2): p. 418-435. 163. T.P. Hoar, D.C.M.a.G.P.R., The production and breakdown of the passivity of metals. Corrosion Science, 1967. 7(6): p. 341-355. 164. K.Y. Ann and H.W.Song., Chloride threshold level for corrosion of steel in concrete Corrosion Science, 2007. 49(11): p. 4113-4133. 165. Y.Zuo, H.W.a.J.X., The aspect ratio of surface grooves and metastable pitting of stainless steel. Corrosion Science, 2002. 44(1): p. 25-35. 166. Y.Zuo, H.W., J. Zhao and J. Xiong, The effects of some anions on metastable pitting of 316L stainless steel Corrosion Science, 2002. 44(1): p. 13-24. 167. M. Duan, H.W., J. Xie, K.P. Yan and Y. Zuo, The nucleation and growth of metastable pitting on pure iron. Corrosion Science, 2009. 51(1): p. 181-185. 168. Z. Szklarska-Smialowska, J.M., Effect of temperature on the kinetics of development of pits in stainless steel in 0.5N NaCl + 0.1N H2SO4 solution. Corrosion Science, 1972. 12(12): p. 925-934. 169. L. Tarja, Localized corrosion of stainless steel in chloride, sulfate and thiosulfate containing environmentsCorrosion Science, 2000.42(3):p.421-441 170. K. Hashimoto, K.A., K. Teramoto, An X-ray photo-electron spectroscopic study on the role of molybdenum in increasing the corrosion resistance of ferritic stainless steels in HCl. science direct, 1979. 19(1): p. 3-14. 171. T. Hong, M.Nagumo., The effect of SO42- concentration in NaCl solution on the early stages of pitting corrosion of type 430 stainless steel Corrosion Science, 1997. 39(5):p.961-967. 172. T. Hong, M.Nagumo., The effect of chloride concentration on early stages of pitting for type 304 stainless steel revealed by the AC impedance method. Corrosion Science, 1997. 39(2): p. 285-293. 173. J.N. Alhajji and M.R. Reda, Role of solution chemistry on corrosion of copper in tap water : Effect of sulfate ion concentration on unifrom and localized attack. NACE, 1996. 52(2): p. 232-238. 174. M.H. Moayed, R.C. Newman, Deterioration in critical pitting temperature of 904L stainless steel by addition of sulfate ions. Corrosion Science, 2006. 48(11): p. 3513-3530. 175. I.L Rosenfeld, I.S.D., Electrochemical aspects of pitting corrosion. Corrosion Science, 1967. 7(3): p. 129-142. 176. M.Piantini, N.D.C., N.Zacchetti, The influence of temperature on the passivation behaviour of a super duplex stainless steel in a boric-borate buffer solution. Corrosion Science, 1997. 39(12): p. 2181-2191. 177. Schumacher, M., Sea water corrosion handbook1979: Noyes Data, New Jersey. 178. B.S. Covino Jr., M.R., T.J. Driscoll, T.C. Murphy, C.R. Molock, The effect of oxygen on the open-circuit passivity of Fe-18Cr Corrosion Science, 1986. 26(2): p. 95-107. 179. H. M. Ezuber, A.E.-H., F. El-Shawesh, Effects of sigma phase precipitation on seawater pitting of duplex stainless steel. science direct, 2007. 207(1-3): p. 268-275. 180. B. Bozzini, M.D., G. P. De Gaudenzi, L. D'Urzo and L. Gregoratti, An investigation of the corrosion of WC–Co cermets in CN--containing aqueous solutions. Part II: Synchrotron-based high lateral-resolution XPS study Corrosion Science, 2009. 51(8): p. 1675-1678. 181. M. Aristizabal, J.M. Sanchez, N. Rodriguez, F. Ibarreta, R. MartinezComparison of the oxidation behaviour of WC–Co and WC–Ni–Co–Cr cemented carbides Corrosion Science, 2011. 53(9): p. 2754-2760. 182. A.Lekatou, E.R., A.E. Karantzalis, Corrosion behaviour of cermet-based coatings with a bond coat in 0.5 M H2SO4. Corrosion Science, 2008. 50(12): p. 3389-3400. 183. C.N. Machio, D.S.KONADU., J. van der Merwe, J.H. Potgieter, S. Potgieter-Vermaak, The corrosion behaviour of WC-VC-Co hardmetals in acidic media. Corrosion Science, 2010. 52(9): pp. 3118-3125. 184. U.Ebersbach, K.S., K. Ritter, On the kineticks of the anodic passivation of iron, cobalt and nickel. Electrchimica Acta, 1967. 12(8): p. 927-938. 185. E.J. Wentzel, C.A., The erosion-corrosion resiatance of tungsten-carbide hard metals. International Journal of Refractory Metals & Hard Materials, 1997. 15(1-3): p. 81-87. 186. S.Virtanen, f.J.J.K., H. Hildebrand, Effect of WC grain size on the corrosion behavior of WC-Co based hardmetals in alkaline solutions. International Journal of Refractory Metals & Hard Materials, 2009. 27: p. 806-812. 187. A.M. Human, H.E.E., The relationship between electrochemical behaviour and in-service corrosion of WC-based cemented carbides. International Journal of Refractory Metals & Hard Materials, 1997. 15(1-3): p. 65-71. 188. G.Gilli, P.B., F.Zucchi, G. Trabanelli, Passivation of Ni caused by layers of salts in concentrated H2SO4. Corrosion Science, 1969. 9(9): p. 673-681. 189. A.Lekatou, D.Z., A.E. Karantzalis, D. Grimanelis, Electrochemical behaviour of cermet coatings with a bond coat on Al7075:Psedopassivatity, localised corrosion and galvanis effect considerations in a saline environment. Corrosion Science, 2010. 52(8): p. 2616-2635. 190. R.B. Perez-Saez, L.d.C., L. Gonzalez-Fernandez, M.J. Tello, Kinetics inversion in isothermal oxidation of uncoated WC-based carbides between 450 and 800 oC. Corrosion Science, 2009. 51(4): p. 707-712. 191. K.S. Indra and K.S.G. Doss. A new approach to explain the anodic passivation and periodic phenomena: The PN junction and SR mechanisms, Central Electrochemical Research Institute , June 3 1967 192. N. J. Laycock. Effects of Temperature and Thiosulfate on Chloride Pitting of Austenitic Stainless Steels,Corrosion June 1999, 55 (6), p. 590-595 193. A. Neville and T. Hodgkiess, An Assessment of the Corrosion Behaviour of High-Grade Alloys in Seawater at Elevated Temperature and Under a High Velocity Impinging Flow, Corrosion Science 1996, 38 (6), p. 927-956 194. M.A. Deyab, Adsorption and inhibition effect of Ascorbyl palmitate on corrosion of carbon steel in ethanol blended gasoline containing water as a contaminant, Corrosion Science 2014, 80, p.359-365 195. W. Li, B. Brown, D. Young and S. Nesic, Investigation of Pseudo-Passivation on mild steel in CO2 corrosion, NACE Corrosion 2013, Paper No. 2149 196 M. Hoseinpoor, M. Momeni, M.H. Moayed and A. Davoodi, EIS assessment of critical pitting temperature of 2205 duplex stainless steel in acidified ferric chloride solution, Corrosion Science 2014, 80,p. 197-204"]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.634276"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/7320/1/Thesis%20final.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["With the increasing demand for environmentally friendly hydraulic fluids in the oil and gas sector, recent advances in hydraulic technology have sparked renewed interest in the application of water instead of oil. For industry, using seawater as a hydraulic fluid would bring many benefits as it can be discharged to the sea. The main corrosion challenges associated with the use of seawater are addressed in this study, particularly on how to extend the material life when corrosion attack is likely to be very severe. On the other hand, the material’s degradation which is common in subsea applications is studied in detail which includes how corrosion mechanisms occur. The materials chosen in this research are those which are used extensively in subsea applications especially in Directional Control Valves (DCV) and piping operating with hydraulic fluids namely: (1) carbon steel, (2) stainless steel, and (3) cermet alloys (WC-Ni and WC-Co). As an active material, carbon steelcorrodes in a general way whereas passive materials such as stainless steel are more prone to localised corrosion which is often more catastrophic and difficult to predict and detect. However, cermets alloys (WC-Ni and WC-Co) which consist of metals and ceramics may exhibit both active and passive trends. Electrochemistry methods which are used in this study provide quantitative data which demonstrates different major corrosion parameters. Generally, temperature, oxygen, anions and pH are the main parameters that affect corrosion attack. In this research the effects of temperature, sulphate to chloride ratio and oxygen were studied on corrosion performance of DCV materials and compared the performance in seawater with a typical commercial hydraulic fluidHW443. From the analysis, it shows that temperature has a severe impact on corrosion rate, but alteration of sulphate to chloride ratio could decrease the corrosion rate close to HW443. Therefore, it is clear that by changing the sulphate/chloride ratio in seawater and adding green corrosion inhibitor similar performance to that compared to the use of commercial hydraulicfluids yet reduce the environmental harm on discharge could be attained. The thesis also presents information ofgeneric interest in corrosion of carbon steel and other materials of interest in subsea environments. Corrosion trends of carbon steel, stainless steel and WC-cermets and their prevalent corrosion mechanisms (from electrochemical analysis) are discussed."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Seawater as a hydraulic fluid; corrosion mechanisms and rates of engineering materials"]}]}],"canonical_facts":{"dc:contributor.advisor":["Neville, Anne"],"dc:contributor.sponsor":["Ministry of Higher Education Malaysia","Aker Solutions, Aberdeen"],"dc:creator":["Ismail, Azzura"],"dc:date":["2014-01"],"dc:date.issued":["2014-01"],"dc:description.abstract":["With the increasing demand for environmentally friendly hydraulic fluids in the oil and gas sector, recent advances in hydraulic technology have sparked renewed interest in the application of water instead of oil. For industry, using seawater as a hydraulic fluid would bring many benefits as it can be discharged to the sea. The main corrosion challenges associated with the use of seawater are addressed in this study, particularly on how to extend the material life when corrosion attack is likely to be very severe. On the other hand, the material’s degradation which is common in subsea applications is studied in detail which includes how corrosion mechanisms occur. The materials chosen in this research are those which are used extensively in subsea applications especially in Directional Control Valves (DCV) and piping operating with hydraulic fluids namely: (1) carbon steel, (2) stainless steel, and (3) cermet alloys (WC-Ni and WC-Co). As an active material, carbon steelcorrodes in a general way whereas passive materials such as stainless steel are more prone to localised corrosion which is often more catastrophic and difficult to predict and detect. However, cermets alloys (WC-Ni and WC-Co) which consist of metals and ceramics may exhibit both active and passive trends. Electrochemistry methods which are used in this study provide quantitative data which demonstrates different major corrosion parameters. Generally, temperature, oxygen, anions and pH are the main parameters that affect corrosion attack. In this research the effects of temperature, sulphate to chloride ratio and oxygen were studied on corrosion performance of DCV materials and compared the performance in seawater with a typical commercial hydraulic fluidHW443. From the analysis, it shows that temperature has a severe impact on corrosion rate, but alteration of sulphate to chloride ratio could decrease the corrosion rate close to HW443. Therefore, it is clear that by changing the sulphate/chloride ratio in seawater and adding green corrosion inhibitor similar performance to that compared to the use of commercial hydraulicfluids yet reduce the environmental harm on discharge could be attained. The thesis also presents information ofgeneric interest in corrosion of carbon steel and other materials of interest in subsea environments. Corrosion trends of carbon steel, stainless steel and WC-cermets and their prevalent corrosion mechanisms (from electrochemical analysis) are discussed."],"dc:format":["text"],"dc:identifier":["uk.bl.ethos.634276"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/7320/1/Thesis%20final.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.commercial":["University of Leeds"],"dc:publisher.department":["Institute of Engineering Thermofluids, Surfaces & Interfaces (iETSI) (Leeds)"],"dc:publisher.institution":["University of Leeds"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/7320/"],"dc:relation.references":["1. Fontana M.G. Corrosion Engineering, McGraw-Hill, 1987, pp. 3-13. 2. Koch, G.H., Michiel P.H. and Thompson N.G.,Corrosion costs and preventive strategies in the United States,Federal Highway Administration (FHWA). FHWA-RD-01-156[online], 2001, [Accessed Jan 2011]. Available from: http://www.corrosioncost.com/summary.htm 3. GuoB., Chacko J.,Ghalambor A., Offshore pipelines. Gulf Professional Publishing[online],2005,p.302. [Accessed October 2008]. Available from: http://books.google.com.my/books/about/Offshore_Pipelines. 4. Chen, M.A.,Influence of hydrolysis time on the structure and corrosion protective performance of (3-mercaptopropyl)triethoxysilane film on copper.Corrosion Science. In Press,2001 5. Mary Tiemann the Specialist in Environmental Policy and Adam Vann, the Legislative Attorney, Hydraulic Fracturing and Safe Drinking Water Act Issues 2 Congressional Research Service, July 12, 201, p.1-42 6. Group, N.E.P.D., Sustainable Development of North America’s Oil and Natural Gas Ensuring Plentiful Energy and a Clean Environment, 2001, Department of Energy: United States of America. p. 3. 7. Azeri, Chirag and Gunashli, Subsea Water Injection Development, 2004, Environmental & Socio Economic Impact Assesment Phase 3 8. Daniel R.S and Newell K.D, Fracturing of Oil and Gas Wells in Kansas, December 2011,Kansas Geological Survey Hydraulic, pp.1-6 9. Knight G.C. 1977, Water hydraulics:Application of water-based fluids to hydraulic systems.Tribology International,10(2): pp. 105-108. 10. Rushau G..R.,Oil and gas exploration and production, 1997. 11. McManus., W.M. Canning Ltd, 1996, Presentations hydraulic fluids for Angola. 12. Zheng, L., Corrosion in hydraulic fluids for subsea applications, in School of Mechanical Engineering2009, University of Leeds: United Kingdom. p. 219. 13. Roberg P.R., Corrosion engineering: Principles and practice: McGraw-Hill, 2008, pp 5, 169-177. 14. KamachiI U. M., Corrosion Science and Technology:Mechanism, Mitigation and Monitoring 2009, Mumbai: narosa publishing house. 15. Denis B., Randy E., Andrew H., Donald H., Shreekant M., and Tony M., Corrosion in the oil industry,Schlumberger Oilfield review[online], 1994, [Accessed 2010]. pp. 1-15.Available from:http://www.slb.com/~/media/Files/resources/oilfield_review/ors94/0494/p04_18.pdf 16. Butler G., H.C.K.I., Corrosion and Its Prevention in Waters1966: A Leonard Hill Book. 281. 17. ToolBox, T.E. Oxygen solubility in fresh and sea water. 2011; Available from: http://www.engineeringtoolbox.com/oxygen-solubility-water-d_841.html. 18. Stansbury E.E. and Buchanan R.A.,Fundamental of electrochemical corrosion, The University of Tennessee, ASM International, 2000. pp 172-197. 19. Shinagawa K, Anti-corrosion Measures for Cable Bearers and Other Iron Fittings in Manholes. NTT Technical Review [online], 2008. 6(11). [Assessed April 2011]. Available from: https://www.ntt-review.jp/archive. 20. Davis J.R., Corrosion:understanding the basics, Ohio, ASM International, 2000, pp 21. Dawson J.L., Corrosion monitoring of steel in concrete in crane. A.P. (ed) corrosion of reinforcement in concrete construction, 1983: p. 175-92. 22. Ahmad Z., Principles of Corrosion Engineering and Corrosion Control. 2006: p. 90-109. 23. Tait W.S., An introduction to electrochemistry corrosion testing for practicing engineers and scientist, 1994, PairODocs Publications. p. 119. 24. Revie R.W., Uhlig's Corrosion Handbook. John Wiley & Sons, 2nd ed, 2000 25. LiI J. et al., Critical pitting and repassivation temperatures for duplex stainless steel in chloride solutions. Electrochimica Acta, 2008. 53(16): p. 5220-5225. 26. Roberge P.R. Handbook of Corrosion Engineering, United States, McGraw Hill, 2008, 27. MalikA.U., Ahmad S., Andijani I.,Corrosion behavior of steels in Gulf seawater environment., Saline Water Conversion Corporation, [online], 1999. 123: pp. 205-213.[Accessed March 2011]. Availabe from : http://www.swcc.gov 28. Roberge P.R. [online]. 2000. [Accessed 19 May 2011]. Availabe from : http://www.corrosion-doctors.org/Forms-crevice/crevice1.htm. 29. FrankelG.S., Sridhar N., Understanding localized corrosion.[online], Materials Today, 2008. 11(10): p. 38-44. [Accessed 2011]. Available from: http://www.matsceng.ohio-state.edu/~frankel/fcc/pubs/data/102.pdf 30. Leckie H.P., UhligH.H., Environmental factor affecting the critical potential for pitting in 18-8 stainless steel.J.Electrochemical Society, 1966. 113(12): p. 1262-1267. 31. Galvele J.R., Transport processes in passivity breakdown-II. Full hydrolysis of the metal ions. Corrosion Science, 1981. 21(8): p. 551-579. 32. Schwenk W, Electrochemical investigations of pitting corrosion.Corrosion Science, 1973. 13(10): pp. 739-746. 33. Sastri V.S, Edward G. and Mimoun E.,Corrosion: Prevention and protection. Practical solutions2007: John Wiley & Sons, Ltd. 34. Watkins J.W. and Kincheloe W., Corrosion of steel in water by varied ratios of dissolved gasses. Corrosion, 1958. 14: p. 341-344. 35. Sridhar N., Brossia C.S, Dunn D.S. and Anderko A., Predicting localized corrosion in seawater. Corrosion, 2004. 60(10): p. 915-936. 36. Uhlig H. H. ,Triadis D.N., and Stern M., Effect of oxygen, chlorides and calcium ion on corrosion inhibition of iron by polyphosphates. J.Electrochemical Society, 1955. 102(2): p. 59-66. 37. CacerasL., Vargas T. and Parra M., Study of the variatonal patterns for corrosion kinetics of carbon steel as a function of dissolved oxygen and NaCl concentration. Electrchimica Acta, 2009. 54: p. 7435-7443. 38. Allen J.B., and Larry R.F., Electrochemical methods, Fundamentals and applications. 2nd ed2001: John WIley & Sons, Inc. 39. Hochstrasser(-Kurz) S.,Mueller Y.,Latkoczy C. and Virtanen S..,Analytical characterization of the corrosion mechanisms of WC–Co by electrochemical methods and inductively coupled plasma mass spectroscopy Corrosion Science, 2007. 49(4): p. 2002-2020. 40. Krkwood D., Microbial corrsion of metals in seawater. proceeding of a meeting organised by the Scottish Marine Biological Association, 1982: p. 16-19. 41. Grobe H. and Majewsky S.,Proportion of salt to sea water and chemical composition of sea salt, Institute for Polar and Marine Research, Bremerhaven, Germany[online], 2008. [Assessed 2009]. Available from: https://wwwalfred Wegener. 42. Mauchline J., Fouling and corrosion of metals in seawater. Science direct, 1982. : p. 281-292. 43. Todd B.,Materials Selection for High Reliability Seawater Systems,Nickel Development Institute[online], 2007. [Assessed 2008]. Available from: http://www.copper.org/applications/cuni/txt_materials_selection.html 44. BrownE., Seawaetr:its composition, properties and behaviour.England, Butterworth Heinemann in association with The Open University, 1999. 2: p. 14-17. 45. Takasaki S. and Yamada.Y., Effects of temperature and aggressive anions on corrosion of carbon steel in potable water. Corrosion Science, 2007. 49(1): p. 240-247. 46. Duthil, J.P., Mankowski, G. and Giusti A.,The synergetic effect of chloride and sulphate on pitting corrosion of copper. Corrosion Science, 1996. 38(10): p. 1839-1849. 47. Abd El Wanees,Abd El Haleem, S.M.,S., Abd El Aal, E.E. and Diab, E., Environmental factors affecting the corrosion behavior of reinforcing steel. IV. Variation in the pitting corrosion current in relation to the concentration of the aggressive and the inhibitive anions,Corrosion Science, 2010. 52(5): pp. 1675-1683. 48. Strehblow H.H. andTitze B., Pitting potentials and inhibition potentials of iron and nickel for different aggressive and inhibiting anions.Corrosion Science, 1977. 17(6). 49. El-Naggar M.M., Effects of Cl−, NO3− and SO42− anions on the anodic behavior of carbon steel in deaerated 0.50 M NaHCO3 solutions,Applied Surface Science, 2006. 252(18). 50. The Hendrix Group Reporter,Hydrogen Embrittlement of High Strength Fasteners![online].1997.7(1), [Accessed 2011], Available from:http://hghouston.com/resources/technical-newsletters/he-of-high-strength-fasteners.aspx 51. Lim, G.H., Chua P.S.K., and He Y.B., Modern water hydraulics--the new energy-transmission technology in fluid power,Applied Energy. 76(1-3): pp. 239-246. 52. Foszcz and Joseph L., \"Hydraulic fluid choices.\" Plant Engineering, 1996. 50(4): p. 68-72. 53. Agency, U.S.E.P., Exemption of oil and gas exploration and production wastes from federal hazardous waste regulations. 53. Knight G.C., Water Hydraulics. Application of water-based fluids to hydraulic systems, Tribology International, April 1977:pp. 105-107. 54. Naylor J. and McManus S., Hydraulic fluids and their future in a more environemntally conscious industry, Martson Bentley report, :. p.1-9 55. Zelman et al., Pipeline and Gas Technology [magazine],November/December 2008, Hart Energy Publishing, LP, p.50 56. Anon, The Centre for Environment, Fisheries & Aquaculture Science (Cefas),[online], 2008, [Assessed June 2011], Available from: http://www.cefas.co.uk/about-us.aspx. 57. Ernest W. K., Use of Corrosion Inhibitors on the Trans Alaska Pipeline, VCI Corrosion ControlSupplement to Materials Performance, January 2001 ORTEC CORP, pp 1-3 58. Ramesh S. and Rajeswari S.,Evaluation of inhibitors and biocide on the corrosion control of copper in neutral aqueous environment. Corrosion Science, 2005. 47(1): pp. 151-169. 59. AlentejanoC.R. and Aoki I.V, Localized corrosion inhibition of 304 stainless steel in pure water by oxyanions tungstate and molybdate. Electrochimica Acta, 2004. 49(17-18): p. 2779-2785. 60. Uhlig H.H., Structure and growth of thin films on metals exposed to oxygen Corrosion Science, 1967. 7(6): pp. 325-339. 61. Gregory R. R and Mohammed A. Al-Anezi., Oil and gas exploration and production. 2000. 62. Dudukcu M., Yazici B. and Erbil M., The effect of indole on the corrosion behaviour of stainless steel. Materials Chemistry and Physics, 2004. 87(1): p. 138-141. 63. Arshadi M.R., Parsafar Gh.A. and Sastri V.S., Cluster/polarized continuum models for density functional theory investigations of benzimidazole corrosion inhibitors at metal/solution interface. NACE International, 2006. 62(3): p. 199-206. 64 DelgadoA. V.,Gonzalez-Caballero F., R., Hunter J., Koopal L.K. and. Yklema J., Measurement and Interpretation of Electrokinetic Phenomena, International Union of Pure and Applied Chemistry Physical Biophysical Chemistry Division, 2005 77(10), pp. 1753–1805 65. Osman M.M., Corrosion inhibition of aluminium-brass in 3.5% NaCl solution and sea water. Materials Chemistry and Physics, 2001. 71(1): pp. 12-16. 66. Hosseini S.M.A., Salari M. and Motlagh M.G,Thioamide compounds as corrosion inhibitors for stainless steel in H2SO4 solution. NACE International, 2010. 66(11): pp. 115003:1-115003:12. 67. YurtA.,Balaban A., Kandemir S.U., Bereket G. and Erk B., Investigation on some Schiff bases as HCl corrosion inhibitors for carbon steel. Materials Chemistry and Physics, 2004. 85(2-3): pp. 420-426. 68. OmanovicS. and Ggreba S, Interaction of 12-aminododecanoic acid with a carbon steel surface:Towards the development of 'green' corrosion inhibitors. Corrosion Science, 2010. 52(6): p. 2104-2113. 69. Sethuraman M.G and.Kamal C., Spirulina platensis-A novel green inhibitor for acud corrosion of mild steel. Arabian Journal of Chemistry, 2010: pp. 1-7. 70. Khaled K.F., Experimental and theoretical study for corrosion inhibitor of mild steel in hydrochloric acid solution by some new hydrazine carbodithioic acid derivatives. Applied Surface Science, 2006. 252(12): p. 4120-4128. 71. Hosseini M.G., Ehteshamzadeh M. and Shahrabi T., Protection of mild steel corrosion with Schiff bases in 0.5 M H2SO4 solution. Electrchimica Acta, 2007. 52(11): p. 3680-3685. 72. LalithaA., Ramesh S. and Rajeswari S., Surface protection of copper in acid medium by azoles and surfactants. Electrchimica Acta, 2005. 51(1): p. 47-55. 73. Saracoglu, M., Zor S., KandemirliF. and ArslanT., Inhibition effects of amides on the corrosion of copper in 1.0 M HCl : Theoretical and experimental studies. NACE International, 2011. 67(12): p. 125003:1-11. 74. Myles M., Jordan N.F., David C.J., Morag and Morag E., Biodegradable scale inhibitors. Laboratory and filed evaluation of \"Green\" carbonate and sulpahte scale inhibitors with deployment histories in the north sea. Chemistry in the oil industry X. Oilfield Chemistry: REACHing the Solution, 2007. 1: pp. 286-308. 75. Division, P.A., The Harmonised Offshore Chemical Notifications Format (HOCNF) Scheme 2006. 76. Wm Canning Ltd, Marston Bentley Division, Cale Lane, Wigan, UK, Technical Manual: OCEANIC HW 600 series: Oceanic HW625, HW 640, HW660: Water based production control fluids for operation of high temperature, high pressure conventional oil and gas wells, 1998,:. 1-58. 77. Manganon P.L., The Principles of Materials Selection for Eingineering Design, Prentice Hall, 1999, pp.512-535. 78. Ueda M., Development of corrosion resistance alloys for the oil and gas industry-based on spontaneous passivity mechanism. NACE International, Corrosion conference, 2006. 62 (10): pp. 856-867. 79. Yang S., Guo J., Shang C. Wang Y. and He X.,Influence of carbon content and microstructure on corrosion behaviour of low alloy steels in a Cl- containing environment, Corrosion Science, 2008. 51 : pp. 242-251. 80. Xu J., Bright M. A., Liu X. and Barbero E., Liquid metal corrosion of 316L stainless steel, 410 stainless steel and 1015 carbon steel in a molten zinc bath, Metallurgical and Materials Transactions A, 2007. 38A: pp.2727-2736. 81. Andijani I. and Turgoose S., Studies on corrosion of carbon steel in deaerated saline solutions in presence of scle inhibitor, Gulf Conference, 1999.: pp. 2231-2246. 82. Lee J. S., Ray R.I., Lemieux E.J., Falster A. U., and Little B. J., An evaluation of carbon steel corrosion under stagnant seawater conditions, Biofouling, 2004. 20 (4/5):. pp. 237-247. 83. Nesmeyanoka, K.A., Effect of oxygen on steel corrosion in steam-water flows at a temperature of 280ºC, Atomnaya Energiya, 1969. 29 (2) :. pp. 781-785. 84. KamachiU.M., and Pujar M.G., Pitting Corrosion of Austenitic Stainless Steels and Their Wekdment. 2002, Narosa Publishing House, pp. 89-91. 85. Smith W.F., Principles of materials science and engineering1996: McGraw Hill. 86. Strafford K.N., Venkatesan K., Subramaniam C. and Green L.K.,Influence of chromium content on corrosion of plasma-nitrided steel, NACE International. 1997,53 (7) :. pp. 507-515. 87. NascimentoD., Ierardi M.C.F, Kina A.Y. and Tavares S.S.M.,Pitting corrosion resistance of cast duplex stainless steels in 3.5%NaCl solution. Materials Characterization, 2008. In Press, Corrected Proof: pp. 1-5. 88. MarcusP., Maurice V.and Strehblow H.H., Localised corrosion (pitting): A modelof passivity breakdown including the role of oxide layer nanostructure. Corrosion Science. 2008, 50:. pp. 2698-2704. 89. Cunha Belo M.D., Rondot B.,Compere C., Montemor M.F., Simões A.M.P., Ferreira M.G.S.,Chemical composition and semiconducting behaviour of stainless steel passive films in contact with artificial seawater. Corrosion Science, 1998. 40(2-3): pp. 481-494. 90. QvarfortR. and Olsson J., Transpassive corrosion of high alloy stainless steels and bickel base alloys, NACE International. 2002. 02133:.pp. 1-17. 91. Fredriksson W., Malmgren S., Gustafsson T., Gorgoi M. and Edstroma K.,Full depth proﬁle of passive ﬁlms on 316L stainless steel based on high resolution HAXPES in combination with ARXPS, Applied Surface Science, 2012. 258:. pp.5790–5797. 92. SouzaE.C., Sergio M., Rossiti and Rollo J.M.D.A Influence of chloride ion concentration and temperature on the electrochemical properties of passive films formed on a superduplex stainless steel. Science Direct, 2010:.pp.240-244. 93. Magellan Metals, Inconel 625[online]. 2004. [Accessed 7 April 2011], Available from: http://www.magellanmetals.com/inconel_625.html?gclid=CNi1v7LJiqgCFUdP4QodrXs6Cw. 94. Cunha Belo D., Hakiki M., Ferreira N.E., Belo M.G.S.,M. C. D and N.E. Hakiki, Semiconducting properties of passive films formed on nickel-base alloys type Alloy 600: infuence of the alloying elements.Electrochimica Acta , 1999, 44 :. pp.2473-2481. 95. WuX. , Huang J. and Han E.H.,,Influence of pH on electrochemical properties of passive films formed on Alloy 690 in high temperature aqueous environments. Corrosion Science, 2009 (51):. pp. 2976-2982. 96. Kawashima A., Asami K. and Hashimoto K.,An XPS study of passive films on nickel and alloy 600 in acids. Corrosion Science. 1985, 25(12):.pp.1103-1114. 97. Yin Z.F., Zhao W.Z., LaiW.Y.and Zhao X.H., Electrochemical behaviour of Ni-base alloys exposed under oi/gas field environments, Corrosion Science. 2009, 51 :.p. 1702-1706 98. Chen C. F., Jiang J., ZhengS.Q.,and Cui L.S.,The non-linear fitting method to study the semiconductor properties of passive films of Inconel alloy G, Journal of Electroanalytical Chemistry, 2011,658 :. p.52–56. 99. Marcus, P., Machet A., Galtayries A., Zanna S., Klein L., Maurice V., Jolivet P, M. Foucault P., Combrade and Scott P.,XPS and STM study of the growth and structure of passive films in high temperature water on a nickel-base alloy, Electrochimica Acta 2004.49 (4):. pp. 3957–3964. 100. YihS.W.H and Wang C.T., Tungsten: sources, metallurgy, properties, and applications1979: Plenum press, New York and London. 358-359. 101. Lekatou A., Zois D., Karantzalis A.E., and Griminelis D., Electrochemical behaviour of cermet coatings with a bond coat on A17075: Psedopassivatity, localized corrosion and galvanic effect considerations in a saline environment, Corrosion Science, 2010, 52, pp. 2616-2635. 102. ViljusM., Klaasena H., Kubarseppa J., Roosaara T., and Traksmaa R., Adhesive wear performance of hardmetals and cermets, Wear, 2010. 268: p. 1122-1128. 103. LacknerA. and Filzwieser A., Gas carburizing of tungsten carbide (WC) powder. U.S Patent 6447742, 2002. 104. Wells, Alexander F., Structural inorganic chemistry. 5 1945: Clarendon Press. p. 590. 105. Scholl H., Hofman B. and Rauscher A., Anodic polarization of cemented carbides of the type [(WC,M): M = Fe, Ni or Co] in sulphuric acid solution..Electrochimica Acta, 1992. 37(3): pp. 447-452. 106. Batchelor A.W., Loh .N.L. and Chandrasekaran M., Materials: Degradation and its control by surface engineering, 2002(2), Singapore: Imperial College Press. p. 412. 107. Upadhayaya G.S., Cemented Tungsten Carbides: Production, Properties, and Testing1998: Noyes Publications. p.403. 108. PotgieterJ.H., Thanjekwayo N., Olubambi P., Maledi N. and Potgieter-Vermaak S.S., Influence of Ru additions on the corrosion behaviour of WC-Co cemented carbide alloys in sufuric acid. Int. Journal of Refractory Metals and Hard Materials, 2011. 29:. pp. 478-487. 109. Buss K. Thesis: High temperature deformation mechanisms of cemented carbides and cermets. Institute of Complex Matter. France, 2004, p 8. 110. TomlinsonW.J. and Linzell C.R.,Anodic polarization and corrosion of cemented carbides with cobalt and nickel binders. Journal of Materials Science, 1988. 23(3): p. 914-918. 111. HumanA.M., Roebuch B. and ExnerH.E., Electrochemical polarization and corrosion behaviour of cobalt and Co (W,C) alloys in 1 N sulphuric acid.. Materials Science and Engineering , 1998. 241: p. 202-210. 112. Anik M.,Effect of concentration gradient on the anodic behavior of tungsten, Science Direct. 2006. 48, pp. 4158-4173. 113. Suleiman A., Skeldon P., Thompson G.E., Echeverria F., Graham M.J., Sproule G.I., Moisa S.,Quance T. and Habazaki H., Anodic oxides on InAlP formed in sodium tungstate electrolyte, Corrosion Science. 2010, 52, pp. 595-601. 114. Lekatou A., Regoutas E., Karantzalis A.E., Corrosion behaviour of cermet-based coatings with a bond coat in 0.5 M H2SO4, Corrosion Science. 2008. 50, pp. 3389-3400. 115. GhandehariM.H. ,Andersen T.N. and Eyring H., The electrochemical reduction of oxygen on copper in dilute sulphuric acid solutions. Corrosion Science, 1976. 16(3): p. 123-135. 116. Sutthiruangwong S. and Mori G., Corrosion properties of Co-based cemented carbides in acidic solutions. International Journals of Refractory Metals & Hard Materials, 2003. 21. pp. 135-145. 117. Warren A., Nylund A and Olefjord I., Oxidation of tungsten and tungsten carbide in dry and humid atmospheres. International Journals of Refractory Metals & Hard Materials, 1996. 14. pp. 345-353 118. Andersson K.M. and Bergstrom L., Oxidation and dissolution of tungsten carbide powder in water,International Journals of Refractory Metals & Hard Materials, 2000. 18. pp. 121-129. 119. Trueman A.R., Schweinsberg D.P. and Hope G.A., A study of the effect of cobalt additions on the corrosion of tungsten carbide/carbon steel metal matrix composites, Corrosion Science, 1999, 41, pp. 1377-1389. 120. Trueman A.R., Schweinsberg D.P., and Hope G.A., The effect of choromium additions on the corrosion behaviour of tungsten carbide/carbon steel metal matrix composites, Corrosion Science, 1998, 40 (10), pp. 1685-1696. 121. KirkovP., The influence of halide ion concentration on the effects of surface active inhibitors in strong electrolytes. Corrosion Science, 1973. 13(10): p. 697-706. 122. Pohjanne P., Carpen L., Kinnunen P., Ramo J., Sarpola A., Riihimaki M., and Hakkarainen T., Stainless steel pitting in chloride-sulfate solutions-the role of cations, 2007, NACE International, Corrosion conference and expo: USA. 123. Pyun P.I, Moon S., Ahn S.H. and Kim S.S.,Effects of Cl-, NO3- and SO42- ions on anodic dissolution of pure aluminium in alkaline solution. Corrosion Science, 1999. 41(4): p. 653-667. 124. Smialowska Z., Effect of the ratio of Cl-/SO42- in solution on the pitting corrosion of Ni. Corrosion Science, 1971. 11(4): p. 209-221. 125. Dechema Handbook of Corrosion, 11 ,Weinheim, NY:VCH Publishers, 1992:. p.66. 126. Hinds G., The electrochemistry of corrosion,[online]. 2006. [Accessed 2012], Available from: http://www.npl.co.uk/upload/pdf/the_electrochemistry 127. Melcher R.E., Effect on marine immersion corrosion of carbon content of low alloy steels. Science direct, 2003. 45(11): p. 2609-2625. 128 Adhikari A.V. and Saliyan V.R.,Quinoline-5-ylmethylene-3-{[8-(trifluromethyl)quinolin-4-yl]thio} propanohydrazide as an effecive inhibitor of mild steel corrosion in HCl solution.. Science direct, 2008. 50. pp.55-61. 129. Christov M. and Popova A., Adsorption characteristics of corrosion inhibitors from corrosion rate measurements.Corrosion Science, 2004. 46. pp.1613-1620. 130. Szklarska-Smialowska Z., The kinetics of pit growth on Ni in solutions with different Cl-/SO42- ratios. Corrosion Science, 1972. 12(6): pp. 527-536. 131. ThompsonN. G. and Payer J.H., DC electrochemical test methods. Vol. 6. 1998. 98. 132. Sedriks A.J., Corrosion stainless steel1979: John Wiley & Sons, New York. 282. 133. Scully J.C., The fundamentals of corrosion1966: Pergamon press. 192. 134. Ziemniak S.E. and Hanson M., Corrosion behavior of 304 stainless steel in high temperature, hydrogenated water. Corrosion Science, 2002. 44(10): p. 2209-2230. 135. Oguzie E.E., Corrosion inhibition of aluminium in acidic and alkaline media by Sansevieria trifasciata extract. Corrosion Science, 2007. 49(3): p. 1527-1539. 136. Stellwag B., The mechanism of oxide film formation on austenitic stainless steels in high temperature water. Corrosion Science, 1998. 40(2/3): p. 337-370. 137. Garfias-Mesias L. F., Sykes J.M.., Metastable pitting in 25 Cr duplex stainless steel. Corrosion Science, 1999. 41(5): p. 959-987. 138. Fischer K. P., SteenslandO., Steinsmo U. and Wallen,B., Comparison of seawater corrosivity in Europe, in EFC1996: UK. 139. Bardal E., Drugli J.M. and Gartland P. O., The behaviour of corrosion-resistant steels in seawater: A review Corrosion Science, 1993. 35(1-4): p. 257-267. 140. Dexter S. C. and Gao G.Y., Corrosion, 1988. 44: p. 717. 141. Laitinen T., Localized corrosion of stainless steel in chloride, sulfate and thiosulfate containing environments. Corrosion Science, 2000. 42(3): p. 421-441. 142. PistoriusP.C. and Burstein G.T., Growth of corrosion pits on stainless steel in chloride solution containing dilute sulphate. Corrosion science, 1992. 33(12): p. 1885-1897. 143. Engqvist H., Beste U. and Axén, N.,International Journal of Refractory Metals and Hard Materials. 2000. 18, 103-109. 144. Hochstrasser(-Kurz) S.,Mueller Y., Latkoczy C.,Virtanen S. and Schmutz P., Analytical characterization of the corrosion mechanisms of WC-Co by electrochemical methods and inductively coupled plasma mass spectrocopy. Corrosion Science, 2007. 49(4): p. 2002-2020. 145. Benedetto, B.,Fanigliulo A. and Mele C., Electrochemical oxidation of WC in acidic sulphate solution Corrosion Science, 2004. 46(2): p. 453-469. 146. Rosales, B.M.Vera, R., and Tapia, C.,Effect of the exposure angle in the corrosion rate of plain carbon steel in a marine atmosphere Corrosion Science, 2003. 45(2): p. 321-337. 147. Zhu, X., Lei, T., Characteristics and formation of corrosion product films of 70Cu-30Ni alloy in seawater. Corrosion Science, 2002. 44(1): p. 67-79. 148. Cáceres, L.,Vargas, T. and Herrera, L.,Determination of electrochemical parameters and corrosion rate for carbon steel in un-buffered sodium chloride solutions using a superposition model. Corrosion Science, 2007. 49(8): p. 3168-3184. 149. Larson, D.T., Surface analytic techniques in corrosion science. Corrosion Science, 1979. 19(10): p. 657-673. 150. Wren,Yazdanfar, K., Zhang, X., Keech, P.G,Shoesmith, D.W.,,Film conversion and breakdown process on carbon steel in the presence of halides. Corrosion Science, 2010. 52(4): p. 1297-1304. 151. Yang, G., Ying, L.,and Haichao, L.,Experimental studies on the local corrosion of low alloy steels in 3.5% NaCl. Corrosion Science, 2001. 43(3): p. 397-411. 152. Jordan, K.G., and Williams V.T., Popeye project: Hydraulic Umbilical, in Offshore Technology Conference, S.O.P. Company, Editor 1996, OTC: Texas. p. 113-120. 153. Melchers, R.E., and Jeffrey, R.,Early corrosion of mild steel in seawater, Corrosion Science, 2005, 47, pp. 1678-1693. 154. Machio, C.N., D.S.KONADU., J. van der Merwe, J.H. Potgieter, S. Potgieter-Vermaak, The corrosion behaviour of WC-VC-Co hardmetals in acidic media. Corrosion Science, 2010. 52(9): pp. 3118-3125. 155. N.J. Laycock, S.E.W., C.A. Johnson, P.T. Wilson, B.J. Webster, Pitting of Type 304 stainless steee in the presence of a biofilm containing sulphate reducing bacteria. Corrosion Science, 1998. 40(2-3): p. 465-480. 156. El-Sayed, A.-R., H.S. Mohran, and H.M. Abd El-Lateef, Potentiodynamic studies on anodic dissolution and passivation of tin, indium and tin-indium alloys in some fruit acids solutions. Corrosion Science, 2009. 51(11): p. 2675-2684. 157. J. Mankowski and Z.Szklarska-Smialowska., Studies on accumulation of chloride ions in pits growing during anodic polarization. Corrosion Science, 1975. 15(6-12): p. 493-501. 158. Jingyi, Z.P.M., Chunchun Xu Youping Liu, Kinetic and thermodynamic behaviour inside occluded corrosion cells interpreted by potential/pH diagrams Corrosion Science, 1989. 29(5): p. 557-566. 159. J.Mankowski, Z.S.-S., Studies on accumulation of chloride ions in pits growing during anodic polarization. Corrosion Science, 1975. 15(6-12): p. 493-501. 160. Wagner, C., Passivity and inhibition during the oxidation of metals at elevated temperatures. Corrosion Science, 1965. 5(11): p. 751-764. 161. Z.F. Yin, W.Z.Z., W.Y. Lai, X.H. Zhao, Electrochemical behaviour of Ni-base alloys exposed under oil/gas field environments. Corrosion Science, 2009. 51(8): p. 1702-1706. 162. Corvo, F., et al., Indoor atmospheric corrosion in Cuba. A report about indoor localized corrosion. Corrosion Science, 2007. 49(2): p. 418-435. 163. T.P. Hoar, D.C.M.a.G.P.R., The production and breakdown of the passivity of metals. Corrosion Science, 1967. 7(6): p. 341-355. 164. K.Y. Ann and H.W.Song., Chloride threshold level for corrosion of steel in concrete Corrosion Science, 2007. 49(11): p. 4113-4133. 165. Y.Zuo, H.W.a.J.X., The aspect ratio of surface grooves and metastable pitting of stainless steel. Corrosion Science, 2002. 44(1): p. 25-35. 166. Y.Zuo, H.W., J. Zhao and J. Xiong, The effects of some anions on metastable pitting of 316L stainless steel Corrosion Science, 2002. 44(1): p. 13-24. 167. M. Duan, H.W., J. Xie, K.P. Yan and Y. Zuo, The nucleation and growth of metastable pitting on pure iron. Corrosion Science, 2009. 51(1): p. 181-185. 168. Z. Szklarska-Smialowska, J.M., Effect of temperature on the kinetics of development of pits in stainless steel in 0.5N NaCl + 0.1N H2SO4 solution. Corrosion Science, 1972. 12(12): p. 925-934. 169. L. Tarja, Localized corrosion of stainless steel in chloride, sulfate and thiosulfate containing environmentsCorrosion Science, 2000.42(3):p.421-441 170. K. Hashimoto, K.A., K. Teramoto, An X-ray photo-electron spectroscopic study on the role of molybdenum in increasing the corrosion resistance of ferritic stainless steels in HCl. science direct, 1979. 19(1): p. 3-14. 171. T. Hong, M.Nagumo., The effect of SO42- concentration in NaCl solution on the early stages of pitting corrosion of type 430 stainless steel Corrosion Science, 1997. 39(5):p.961-967. 172. T. Hong, M.Nagumo., The effect of chloride concentration on early stages of pitting for type 304 stainless steel revealed by the AC impedance method. Corrosion Science, 1997. 39(2): p. 285-293. 173. J.N. Alhajji and M.R. Reda, Role of solution chemistry on corrosion of copper in tap water : Effect of sulfate ion concentration on unifrom and localized attack. NACE, 1996. 52(2): p. 232-238. 174. M.H. Moayed, R.C. Newman, Deterioration in critical pitting temperature of 904L stainless steel by addition of sulfate ions. Corrosion Science, 2006. 48(11): p. 3513-3530. 175. I.L Rosenfeld, I.S.D., Electrochemical aspects of pitting corrosion. Corrosion Science, 1967. 7(3): p. 129-142. 176. M.Piantini, N.D.C., N.Zacchetti, The influence of temperature on the passivation behaviour of a super duplex stainless steel in a boric-borate buffer solution. Corrosion Science, 1997. 39(12): p. 2181-2191. 177. Schumacher, M., Sea water corrosion handbook1979: Noyes Data, New Jersey. 178. B.S. Covino Jr., M.R., T.J. Driscoll, T.C. Murphy, C.R. Molock, The effect of oxygen on the open-circuit passivity of Fe-18Cr Corrosion Science, 1986. 26(2): p. 95-107. 179. H. M. Ezuber, A.E.-H., F. El-Shawesh, Effects of sigma phase precipitation on seawater pitting of duplex stainless steel. science direct, 2007. 207(1-3): p. 268-275. 180. B. Bozzini, M.D., G. P. De Gaudenzi, L. D'Urzo and L. Gregoratti, An investigation of the corrosion of WC–Co cermets in CN--containing aqueous solutions. Part II: Synchrotron-based high lateral-resolution XPS study Corrosion Science, 2009. 51(8): p. 1675-1678. 181. M. Aristizabal, J.M. Sanchez, N. Rodriguez, F. Ibarreta, R. MartinezComparison of the oxidation behaviour of WC–Co and WC–Ni–Co–Cr cemented carbides Corrosion Science, 2011. 53(9): p. 2754-2760. 182. A.Lekatou, E.R., A.E. Karantzalis, Corrosion behaviour of cermet-based coatings with a bond coat in 0.5 M H2SO4. Corrosion Science, 2008. 50(12): p. 3389-3400. 183. C.N. Machio, D.S.KONADU., J. van der Merwe, J.H. Potgieter, S. Potgieter-Vermaak, The corrosion behaviour of WC-VC-Co hardmetals in acidic media. Corrosion Science, 2010. 52(9): pp. 3118-3125. 184. U.Ebersbach, K.S., K. Ritter, On the kineticks of the anodic passivation of iron, cobalt and nickel. Electrchimica Acta, 1967. 12(8): p. 927-938. 185. E.J. Wentzel, C.A., The erosion-corrosion resiatance of tungsten-carbide hard metals. International Journal of Refractory Metals & Hard Materials, 1997. 15(1-3): p. 81-87. 186. S.Virtanen, f.J.J.K., H. Hildebrand, Effect of WC grain size on the corrosion behavior of WC-Co based hardmetals in alkaline solutions. International Journal of Refractory Metals & Hard Materials, 2009. 27: p. 806-812. 187. A.M. Human, H.E.E., The relationship between electrochemical behaviour and in-service corrosion of WC-based cemented carbides. International Journal of Refractory Metals & Hard Materials, 1997. 15(1-3): p. 65-71. 188. G.Gilli, P.B., F.Zucchi, G. Trabanelli, Passivation of Ni caused by layers of salts in concentrated H2SO4. Corrosion Science, 1969. 9(9): p. 673-681. 189. A.Lekatou, D.Z., A.E. Karantzalis, D. Grimanelis, Electrochemical behaviour of cermet coatings with a bond coat on Al7075:Psedopassivatity, localised corrosion and galvanis effect considerations in a saline environment. Corrosion Science, 2010. 52(8): p. 2616-2635. 190. R.B. Perez-Saez, L.d.C., L. Gonzalez-Fernandez, M.J. Tello, Kinetics inversion in isothermal oxidation of uncoated WC-based carbides between 450 and 800 oC. Corrosion Science, 2009. 51(4): p. 707-712. 191. K.S. Indra and K.S.G. Doss. A new approach to explain the anodic passivation and periodic phenomena: The PN junction and SR mechanisms, Central Electrochemical Research Institute , June 3 1967 192. N. J. Laycock. Effects of Temperature and Thiosulfate on Chloride Pitting of Austenitic Stainless Steels,Corrosion June 1999, 55 (6), p. 590-595 193. A. Neville and T. Hodgkiess, An Assessment of the Corrosion Behaviour of High-Grade Alloys in Seawater at Elevated Temperature and Under a High Velocity Impinging Flow, Corrosion Science 1996, 38 (6), p. 927-956 194. M.A. Deyab, Adsorption and inhibition effect of Ascorbyl palmitate on corrosion of carbon steel in ethanol blended gasoline containing water as a contaminant, Corrosion Science 2014, 80, p.359-365 195. W. Li, B. Brown, D. Young and S. Nesic, Investigation of Pseudo-Passivation on mild steel in CO2 corrosion, NACE Corrosion 2013, Paper No. 2149 196 M. Hoseinpoor, M. Momeni, M.H. Moayed and A. Davoodi, EIS assessment of critical pitting temperature of 2205 duplex stainless steel in acidified ferric chloride solution, Corrosion Science 2014, 80,p. 197-204"],"dcterms:accessrights":["public"],"dc:title":["Seawater as a hydraulic fluid; corrosion mechanisms and rates of engineering materials"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"]},"updated_at":"2026-11-18T21:28:06Z"}