{"id":{"repo_id":"whiterose","oai_identifier":"oai:etheses.whiterose.ac.uk:7329"},"canonical_url":"https://search.ndltd.org/etd/whiterose/oai:etheses.whiterose.ac.uk:7329","repository":{"repo_id":"whiterose","name":"White Rose University Consortium","base_url":"https://etheses.whiterose.ac.uk/cgi/oai2"},"display":{"title":"Corrosion processes and mechanisms in the presence of MonoEthylene Glycol (MEG)","abstract":"Carbon steel pipelines are employed in the oil and gas industry for long distance multiphase transportation. The integrity of these pipelines is critical to oil and gas production. Transportation of wet natural gas using carbon steel pipelines from source to processing plant may lead to corrosion, hydrate formation and even scale formation. To prevent hydrate formation MonoEthylene Glycol (MEG) is pumped through the pipeline. Corrosion inhibitors and other corrosion prevention methods may be employed to reduce corrosion to manageable and acceptable levels. In this study the corrosion inhibition properties of MEG were investigated at both low and high temperature conditions. The reduction of carbon steel X65 corrosion in the presence of MEG alone and 1% NaCl alone at low temperature of 20°C was in line with previous studies. At high temperature of 80°C, the corrosion rate of the carbon steel in the presence of MEG tends to increase. Thus the reduction of the corrosion rate of carbon steel in the presence of MEG can be underestimated. The increase in the corrosion rate of carbon steel in the presence of MEG at high temperature led to the search for the mechanism by which MEG reduces corrosion. The adsorption process was studied using Fourier transform infra-red spectroscopy (FTIR). Further determination of the adsorption isotherm properties and behaviour of MEG on the corrosion of carbon steel was recorded through experimentation. The results were used to determine the type of adsorption that occurs in the presence of MEG. The corrosion rate of carbon steel in the presence of MEG is improved by deployment of chemical inhibitors to reach a minimal acceptable rate. This study investigated the use of two types of commercially-available inhibitors green (inhibitor 2) and non-green inhibitor (inhibitor 1) for reduction of the corrosion rate. The effects of the two inhibitors alone on the corrosion of carbon steel at both high and low temperatures were first examined. This enabled an assessment of the inhibitor in the presence of MEG. A combination of the MEG and inhibitor was tested at both low and high concentrations. The influence on MEG on the inhibitor performance was determined. Conditions necessary for the formation of protective iron carbonate were determined and used for pre-corrosion. The influence of iron carbonate on the corrosion of carbon steel was determined. Pre-corroded carbon steel was used to assess the influence of MEG in the presence of iron carbonate. Further test on the pre-corroded carbon steel in the presence of MEG and inhibitor was performed to assess the influence of the inhibitor and MEG on iron carbonate scale.","abstract_html":"Carbon steel pipelines are employed in the oil and gas industry for long distance multiphase transportation. The integrity of these pipelines is critical to oil and gas production. Transportation of wet natural gas using carbon steel pipelines from source to processing plant may lead to corrosion, hydrate formation and even scale formation. To prevent hydrate formation MonoEthylene Glycol (MEG) is pumped through the pipeline. Corrosion inhibitors and other corrosion prevention methods may be employed to reduce corrosion to manageable and acceptable levels. In this study the corrosion inhibition properties of MEG were investigated at both low and high temperature conditions. The reduction of carbon steel X65 corrosion in the presence of MEG alone and 1% NaCl alone at low temperature of 20°C was in line with previous studies. At high temperature of 80°C, the corrosion rate of the carbon steel in the presence of MEG tends to increase. Thus the reduction of the corrosion rate of carbon steel in the presence of MEG can be underestimated. The increase in the corrosion rate of carbon steel in the presence of MEG at high temperature led to the search for the mechanism by which MEG reduces corrosion. The adsorption process was studied using Fourier transform infra-red spectroscopy (FTIR). Further determination of the adsorption isotherm properties and behaviour of MEG on the corrosion of carbon steel was recorded through experimentation. The results were used to determine the type of adsorption that occurs in the presence of MEG. The corrosion rate of carbon steel in the presence of MEG is improved by deployment of chemical inhibitors to reach a minimal acceptable rate. This study investigated the use of two types of commercially-available inhibitors green (inhibitor 2) and non-green inhibitor (inhibitor 1) for reduction of the corrosion rate. The effects of the two inhibitors alone on the corrosion of carbon steel at both high and low temperatures were first examined. This enabled an assessment of the inhibitor in the presence of MEG. A combination of the MEG and inhibitor was tested at both low and high concentrations. The influence on MEG on the inhibitor performance was determined. Conditions necessary for the formation of protective iron carbonate were determined and used for pre-corrosion. The influence of iron carbonate on the corrosion of carbon steel was determined. Pre-corroded carbon steel was used to assess the influence of MEG in the presence of iron carbonate. Further test on the pre-corroded carbon steel in the presence of MEG and inhibitor was performed to assess the influence of the inhibitor and MEG on iron carbonate scale.","abstract_has_math":false,"creators":["Ivonye, Ikechukwu C."],"institution":"University of Leeds","degree_name":"Ph.D","degree_level":"doctoral","degree_discipline":null,"degree_department":null,"school":null,"contributors":[],"advisors":["Neville, Anne","Wang, Chun"],"committee_chairs":[],"committee_members":[],"year":2014,"date_issued":"2014-07","date_published":"2014-07","updated_at":"2026-11-18T21:28:19Z","subjects":[],"languages":["eng"],"rights":[],"rights_urls":[],"identifier_entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.635382"],"render_values":[{"text":"uk.bl.ethos.635382","href":null,"code":true}]}],"person_identifier_entries":[]},"links":{"outbound_url":null,"outbound_label":null,"outbound_source":null,"record_url":null,"record_label":null,"record_kind":null,"record_source":null,"download_url":"https://etheses.whiterose.ac.uk/id/eprint/7329/1/Ikechukwu%20C.%20Ivonye%20Thesis.pdf","download_label":"Download PDF","download_source":"dc:identifier.uri","access_status":null,"embargo_until":null,"access_note":null},"source_record":{"url":"https://etheses.whiterose.ac.uk/cgi/oai2?verb=GetRecord&metadataPrefix=uketd_dc&identifier=oai%3Aetheses.whiterose.ac.uk%3A7329","prefix":"uketd_dc"},"metadata_groups":[{"id":"people","label":"People","entries":[{"key":"dc:contributor.advisor","label":"Advisor","values":["Neville, Anne","Wang, Chun"]},{"key":"dc:creator","label":"Author","values":["Ivonye, Ikechukwu C."]}]},{"id":"academic_context","label":"Academic Context","entries":[{"key":"dc:date","label":"Dc Date","values":["2014-07"]},{"key":"dc:date.issued","label":"Date","values":["2014-07"]},{"key":"dc:publisher.commercial","label":"Dc Publisher Commercial","values":["University of Leeds"]},{"key":"dc:publisher.department","label":"Dc Publisher Department","values":["School of Mechanical Engineering (Leeds)","Institute of Engineering Thermofluids, Surfaces & Interfaces (iETSI) (Leeds)"]},{"key":"dc:publisher.institution","label":"Dc Publisher Institution","values":["University of Leeds"]},{"key":"dc:relation.isreferencedby","label":"Dc Relation Isreferencedby","values":["https://etheses.whiterose.ac.uk/id/eprint/7329/"]},{"key":"dc:relation.references","label":"Dc Relation References","values":["1. Christof, R. BP Energy Outlook 2035 2014 [cited 2014 21/03/2014]; 4th edition:[Available from: http://www.bp.com/en/global/corporate/about-bp/energy-economics/energy-outlook.html?gclid=CMWg5YyXpL0CFS7MtAodiVIAKg. 2. Brustad, S., K.-P. Løken, and J.G. Waalmann, Hydrate Prevention using MEG instead of MeOH: Impact of experience from major Norwegian developments on technology selection for injection and recovery of MEG, in Offshore Technology Conference. 2005: Houston, Texas. 3. L.Fosb, P., K. Thomsen, and E. H.Stenby, Improving Mechanistic CO2 Corrosion Models in CORROSION 2009. 2009, NACE International: Atlanta, GA. 4. Revie, R.W., Uhlig H. Herbert, Corrosion and Corrosion Control : An Introduction to Corrosion Science and Engineering. 4th ed. 2008, Hoboken, N.J.: J. Wiley. 5. G.H.Koch, M.P.H.B., N.G.Thompson,Y.P.Virmani, and J.H.Payer, Corrosion Cost and Preventon Strategies in the United States,. 2002, Federal highway administration, U.S. Department of Transportation: McLean VA. 6. Papavinasam, S., Corrosion Control in the Oil and Gas Industry. 2014, London, UK: Elsevier Inc. 7. Utility Board (ERCB) 91-G Report 2007, Alberta Energy Regulator (AER): 250-5th street SW, Calgary, Alberta, Canada,. 8. Wang, C., Erosion-Corrosion Mitigation Using Chemicals, in School of Mechanical Engineering. 2007: University of Leeds. 9. Barker, R.J., Erosion-Corrosion of Carbon Steel Pipework on an Offshore Oil and Gas facility, in School of Mechanical Engineering. 2012, University of Leeds: University of Leeds. 10. R.A.Buchanan, E.E.S.a., Fundamentals of Electrochemical Corrosion. 2000, Ohio: ASM International. 11. Tait, W.S., ed. An Introduction to Electrochemical Corrosion Testing for Practicing Engineers and Scientists. 1994, Racine, WI: Pair O Docs Publications. 12. Ren, C.Q., et al., Corrosion Behavior of Oil Tube Steel in Simulant Solution with Hydrogen Sulfide and Carbon Dioxide. Materials Chemistry and Physics, 2005. 93(2-3): p. 305-309. 13. ; Available from: http://chemwiki.ucdavis.edu/Analytical_Chemistry/Analytical_Chemistry_2.0/11_Electrochemical_Methods/11B_Potentiometric_Methods. 14. Sastri, V.S., Corrosion Prevention and Protection : Practical Solutions. 2007, Chichester: Wiley. 15. Revie, R.W., Uhlig's Corrosion Handbook. 2nd ed. 2000, New York: Wiley. 16. Thomas, J., The Mechanism of Corrosion Prevention by Inhibitors, in Corrosion Control, L.L.Shreir, Editor. 1979, Newnes-Butterworths: Uk. 17. Sastri, V.S., Corrosion Inhibitors : Principles and Applications 1998, Chichester ; New York :: Wiley. 18. Denzine, A.F. and M.S. Reading, A Critical Comparison of Corrosion Monitoring Techniques used in Industrial applications, in Corrosion97. 1997, NACE International: New Orleans, LA. 19. Scully, J.R., The Polarization Resistance Method for Determination of Instantaneous Corrosion Rates: A Review, in CORROSION 98. 1998, NACE International: San Diego Ca. 20. Scully, J.R., Polarization Resistance Method for Determination of Instantaneous Corrosion Rates. Corrosion, 2000. 56(2): p. 199-218. 21. Nesic, S., Key Issues Related to Modelling of Internal Corrosion of Oil and Gas Pipelines - A Review. Corrosion Science, 2007. 49(12): p. 4308-4338. 22. Sun, W., S. Nesic, and R.C. Woollam, The Effect of Temperature and Ionic Strength on Iron Carbonate (FeCO3) Solubility limit. Corrosion Science, 2009. 51(6): p. 1273-1276. 23. Wang, X., et al., Comprehensive Study of the Hydration and Dehydration Reactions of Carbon Dioxide in Aqueous Solution. The Journal of Physical Chemistry A, 2009. 114(4): p. 1734-1740. 24. Alberty, R., Physical Chemistry. 1983: John Wiley and Sons 25. Bruno, J., The Influence of Dissolved Carbon dioxide on Trace Metal Speciation in Seawater. Marine Chemistry, 1990. 30(0): p. 231-240. 26. Palmer, D.A. and R. Van Eldik, The Chemistry of Metal Carbonato and Carbon dioxide Complexes. Chemical Reviews, 1983. 83(6): p. 651-731. 27. Nesic, S., et al., An Open Source Mechanistic Model for CO2 /H2S Corrosion of Carbon Steel, in CORROSION 2009. 2009, NACE International: Atlanta, GA. 28. Schmitt, G. and M. Horstemeier, Fundamental Aspects of CO2 Metal Loss Corrosion - Part II: Influence of Different Parameters on CO2 Corrosion Mechanisms, in Corrosion 2006. 2006, NACE International: San Diego Ca. 29. J. O'M. Bockris, N.B., F. Gutmann, An Introduction to Electrochemical Science 1974, London Wykeham Publications. 30. J.O.M. Bockris, D.D., A.R. Despic, , The Electrode Kinetics of the Deposition and Dissolution of iron. Electrochemica acta, 1965. 4: p. 325-361. 31. J.O.M. Bockris, D.M.D., Electro-Chemical Science. 1972, Taylor and Francis: London. 32. Nesic, S., J. Postlethwaite, and S. Olsen, An Electrochemical Model for Prediction of Corrosion of Mild Steel in Aqueous Carbon Dioxide Solutions. Corrosion, 1996. 52(04). 33. Dugstad, A., Mechanism of Protective Film Formation During CO2 Corrosion of Carbon Steel, in CORROSION 98. 1998, NACE International: San Diego Ca. 34. Nyborg, R., Overview of CO2 Corrosion Models for Wells and Pipelines, in CORROSION 2002. 2002, NACE International: Denver, Co. 35. Kermani, M.B. and A. Morshed, Carbon Dioxide Corrosion in Oil and Gas ProductionA Compendium. Corrosion, 2003. 59(08). 36. de Waard, C. and D.E. Milliams, Carbonic Acid Corrosion of Steel. Corrosion, 1975. 31(5): p. 177-181. 37. Hurlen, T., Corrosion of Iron-Effect of pH and Ferrous Ion Activity Acta Chemica Scandinavica, 1960. 14(7): p. 1555-1563. 38. L.G.S. Gray, B.G.A., M.J. Danysh, P.G. Tremaine, , Mechanism of Carbon Steel Corrosion in Brines Containing Dissolved Carbon Dioxide at pH 4, in Corrosion89. 1989, NACE: Houston Tx. 39. L.G.S. Gray, B.G.A., M.J. Danysh, P.R. Tremaine, , Effect of pH and Temperature on the Mechanism of Carbon Steel Corrosion by Aqueous Carbon dioxide, in NACE International. 1990, NACE: Houston Tx. 40. Nesic, S., et al., Electrochemical Properties of Iron Dissolution in the Presence of CO2 - Basics Revisited, in CORROSION 96. 1996, NACE International: Denver, Co. 41. Dewaard, C. and D.E. Milliams, CARBONIC-ACID CORROSION OF STEEL. Corrosion, 1975. 31(5): p. 177-181. 42. Schmitt, G. and B. Rothmann, Investigations into Corrosion Mechanism of Unalloyed Steel in Oxygen-Free Carbonic-Acid Solutions .1. Kinetics of Hydrogen Evolution. Werkstoffe Und Korrosion-Materials and Corrosion, 1977. 28(12): p. 816-822. 43. Schmitt, G. and B. Rothmann, Investigations into Corrosion of Mild-Steel in Oxygen-Free Carbon-dioxide Solutions.2. Kinetic of Iron Dissolution. Werkstoffe Und Korrosion-Materials and Corrosion, 1978. 29(2): p. 98-100. 44. Schmitt, G. and B. Rothmann, Corrosion of Unalloyed and Low Alloyed Steels in Carbonic-Acid Solutions. Werkstoffe Und Korrosion-Materials and Corrosion, 1978. 29(4): p. 237-245. 45. Ogundele, G.I. and W.E. White, Some Observations on Corrosion of Carbon-Steel in Aqueous Environments Containing Carbon-dioxide. Corrosion, 1986. 42(2): p. 71-78. 46. Mora-Mendoza, J.L. and S. Turgoose, Influence of Turbulent Flow on the Localized Corrosion Processes of Mild Steel With Inhibited Aqueous CO2 Systems, in CORROSION 2001. 2001, NACE International: Houston, Tx. 47. Postlethwaite, J. and D. Wang, Modeling Aqueous CO2 Corrosion of Iron in Turbulent Pipe Flow, in Corrosion 2001. 2001, NACE International: Houston, Texas. 48. Nesic, S., G.T. Solvi, and J. Enerhaug, Organic Materials Generally are Recognized as Effective Inhibitors of the Corrosion of Many Metals and Alloys. Corrosion, 1995. 51(10). 49. Videm, K. and A.M. Koren, Corrosion, Passivity, and Pitting of Carbon-Steel in Aqueous-Solutions of HCO3 -, CO2, and Cl- Corrosion, 1993. 49(9): p. 746-754. 50. K.Videm, A.D., Corrosion of Carbon Steel in an Aqueous Carbon dioxide Environment. Part 2. Film Formation,. material Performance, 1989. 28: p. 46-50. 51. Ikeda, A., S. Mukai, and M. Ueda, Relationship Between Environmental-factors and Corrosion Product on CO2 Corrosion. Transactions of the Iron and Steel Institute of Japan, 1984. 24(12): p. B401-B401. 52. Ikeda, A., CO2 Corrosion of Iron and Steel in Oil and Gas Production. Journal of the Japan Petroleum Institute, 2002. 45(2): p. 55-69. 53. de Waard, C., U. Lotz, and D.E. Milliams, Predictive Model for CO2 Corrosion Engineering in Wet Natural Gas Pipelines. Corrosion, 1991. 47(12): p. 976-985. 54. Palacios, C.A.a.S., J.R., Characteristics of Corrosion Scales on Steel in a CO2-Saturated NaCl Brine. Corrosion, 1991. 47(2): p. 122-127. 55. Papavinasam, S., A. Doiron, and R.W. Revie, Effect of Surface Layers on the Initiation of Internal Pitting Corrosion in Oil and Gas Pipelines. Corrosion, 2009. 65(10): p. 663-673. 56. Papavinasam, S., A. Doiron, and R.W. Revie, Model to Predict Internal Pitting Corrosion of Oil and Gas Pipelines. Corrosion, 2010. 66(3). 57. Nyborg, R. and A. Dugstad, Understanding and Prediction of Mesa Corrosion Attack, in CORROSION 2003. 2003, NACE International: San Diego Ca. 58. Schmitt, G.A., et al., Understanding Localized CO2 Corrosion of Carbon Steel from Physical Properties of Iron Carbonate Scales, in Corrosion99. 1999, NACE International: San Antonio, Texas. 59. Heuer, J.K. and J.F. Stubbins, An XPS Characterization of FeCO3 Films from CO2 Corrosion. Corrosion Science, 1999. 41(7): p. 1231-1243. 60. John, R.C., et al., SweetCor: An Information System for the Analysis of Corrosion of Steels by Water and Carbon Dioxide, in CORROSION 98. 1998, NACE International: San Diego Ca. 61. Xia, Z., K.C. Chou, and Z. Szklarskasmialowska, Pitting Corrosion of Carbon-Steel in CO2-Containing Nacl Brine. Corrosion, 1989. 45(8): p. 636-642. 62. Farelas, F., B. Brown, and S. Nesic, Iron Carbide and its Influence on the Formation of Protective Iron Carbonate in CO2 Corrosion of Mild Steel, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 63. J-L.Crolet and M.R.Bonis, Alogorithm of the Protectiveness of Corrosion Layers 1-Protectiveness Mechanism and CO2 Corrosion Prediction, in Corrosion 2010. 2010, NACE International: San Antonio, Texas. 64. Crolet, J.L., N. Thevenot, and S. Nesic, Role of Conductive Corrosion Products in the Protectiveness of Corrosion Layers. Corrosion, 1998. 54(03). 65. Crolet, J.L., S. Nesic, and N. Thevenot, Role of Conductive Corrosion Products on the Protectiveness of Corrosion Layers, in CORROSION 96. 1996, NACE International: Denver, Co. 66. De Waard, C., U. lotz, and A. Dugstad, Influence of Liquid Flow Velocity on CO2 Corrosion: A Semi-Emprical Model, in Corrosion 95. 1995, NACE USA. 67. De Waard, C. and U. lotz, Prediction of CO2 Corrosion of Carbon Steel, in Corrosion 93. 1993, NACE: USA. 68. Harris, M.G., M.C.D. Adams, and D.J.D. Garber, Use of a Corrosion Prediction Program as an Engineering Tool, in Corrosion97. 1997, NACE International: New Orleans, LA. 69. Woollam, R.C. and S. Hernandez, Assessment and comparison of CO2 corrosion predicition models, in SPE International Oilfield Corrosion Symposium. 2006: Aberdeen, UK. 70. Hunnik, E.V., B.F.M. Pots, and E.L.J.A. Hendriksen, The Formation of Protective Fe3CO2 Corrosion Product Layers in CO Corrosion, in Corrosion96. 1996, NACE International: Denver, Colorado. 71. Pots, B.F.M., Mechanistic Models for the Prediction of CO2 Corrosion Rates Under Multi-Phase Flow Conditions, in CORROSION. 1995, NACE. 72. Nyborg, R., A. Dugstad, and L. Lunde, Corrosion and Glycol Distribution in a Large Wet-Gas Pipeline. Materials Performance, 1993. 32(9): p. 57-61. 73. Ayello, F.x.o., et al., Determination of Phase Wetting in Oil-Water Pipe Flows in CORROSION 2008. 2008, NACE International: New Orleans LA. 74. M. Wicks, J.P.F.M., Material Performance, 1975. 9. 75. Halvorsen, A.M. and T. Sontvedt, CO2 Corrosion Model for Carbon Steel Including Wall Shear Stress Model for Multiphase Flow and Limits for Production Rate to Avoid Mesa Attack, in CORROSION 99. 1999, NACE International: San Antonio, Tx. 76. Adams, C.D., et al., Computer Modeling to Predict Corrosion Rates in Gas Condensate Wells Containing CO2, in CORROSION 96. 1996, NACE International: Denver, Co. 77. Dugstad, A., M. Seiersten, and R. Nyborg, Flow Assurance of pH Stabilized Wet Gas Pipelines, in CORROSION 2003. 2003, NACE International: San Diego Ca. 78. Sun, W. and S. Nesic, Kinetics of Corrosion Layer Formation: Part 1 - Iron Carbonate Layers in Carbon dioxide Corrosion. Corrosion, 2008. 64(4): p. 334-346. 79. Dugstad, A., Formation of Protective Corrosion Films during CO2 Corrosion of Carbon Steel. Advances in Corrosion Control and Materials in Oil and Gas Production, 1999(26): p. 70-76. 80. J.L.Crolet, S.O., W.Wilhelmsen, Influence of a Layer of Indissolved Cementite on the Rate of the CO2 Corrosion of Carbon steel, in Corrosion94. 1994: Houston, Tx. 81. Seal, S., et al., The Effect of Flow on the Corrosion Product Layer in Presence of Corrosion Inhibitors, in CORROSION 2002. 2002, NACE International: Denver, Co. 82. Wang, H., et al., Why Corrosion Inhibitors Do Not Perform Well in Some Multiphase Conditions: A Mechanistic Study, in Corrosion 2002. 2002, NACE International: Denver, Colorado. 83. Chen, H.J. and W.P. Jepson, Inhibition of Slug Front Corrosion in Multiphase Flow Conditions, in CORROSION 98. 1998, NACE International: San Diego Ca. 84. Al-Hassan, S., et al., Effect of Microstructure on Corrosion of Steels in Aqueous Solutions Containing Carbon Dioxide. Corrosion, 1998. 54(06). 85. Dugstad, A., H. Hemmer, and M. Seiersten, Effect of Steel Microstructure on Corrosion Rate and Protective Iron Carbonate Film Formation. Corrosion, 2001. 57(04). 86. Dugstad, A. and P.-E. Dronen, Efficient Corrosion Control of Gas Condensate Pipelines by pH - Stabilization, in Corrosion 99. 1999, NACE International. 87. Gulbrandsen, E. and J.H. Morard, Why Does Glycol Inhibit CO2 Corrosion?, in CORROSION 98. 1998, NACE International: San Diego Ca. 88. Garsany, Y., D. Pletcher, and B.M. Hedges, The Role of Acetate in CO2 Corrosion of Carbon Steel: Has the Chemistry Been Forgotten?, in Corrosion 2002. 2002, NACE International: Denver, Colorado. 89. Garsany, Y., et al., Quantifying the Acetate-Enhanced Corrosion of Carbon Steel in Oilfield Brines, December 2004. Corrosion, 2004. 60(12). 90. Sun, Y., K. George, and S. Nesic, The Effect of Cl- and Acetic Acid on Localized CO2 Corrosion in Wet Gas Flow, in Corrosion 2003. 2003, NACE International: San Diego Ca. 91. George, K., K.d. Waard, and S. Nesic, Electrochemical Investigation and Modeling of Carbon Dioxide Corrosion of Carbon Steel in the Presence of Acetic Acid. 2004, NACE International. 92. Crolet, J.L., A. Dugstad, and N. Thevenot, Role of Free Acetic Acid on the CO2 Corrosion of Steels, in CORROSION 99. 1999, NACE International: San Antonio, Tx. 93. Gulbrandsen, E. and K. Bilkova, Solution Chemistry Effects on Corrosion of Carbon Steels in Presence of CO2 and Acetic Acid, in Corrosion 2006. 2006, NACE International: San Diego, California. 94. Nafday, O. and S. Nesic, Iron Carbonate Scale Formation and CO2 Corrosion in the Presence of Acetic Acid, in Corrosion 2005. 2005, NACE International: Houston, Texas. 95. Wheeler, P.J., lntroduction to the Troll Project, in OTC 97. 1997, Offshore Technology Conference: Houston, Texas. 96. Rebsdat, S. and D. Mayer, Ethylene Glycol, in Ullmann's Encyclopedia of Industrial Chemistry. 2000, Wiley-VCH Verlag GmbH & Co. KGaA. 97. Rebsdat, S. and D. Mayer, ETHYLENE GLYCOL. Gerhartz, W., Et Al. (Ed.). Ullmann's Encyclopedia of Industrial Chemistry, Fifth Completely Revised Edition, Vol. A 10. Ethanolamines to Fibers, 4. Synthetic Organic. Xv+655p. Vch Publishers, Inc.: New York, New York, USA; Cambridge, England, Uk; Vch Verlagsgesellschaft Mbh: Weinheim, West Germany. Illus. Maps, 1987: p. 101-116. 98. Boxall, J., et al., Predicting When and Where Hydrate Plugs Form in Oil-Dominated Flowlines. SPE Projects, Facilities & Construction, 2009. 4(3): p. pp. 80-86. 99. Elhady, A.A.A., Operating Experiences of DEG and MEG for Hydrate and Dew Point Control in Gas Production Offshore Mediterranean, in International Petroleum Technology Conference. 2005, International Petroleum Technology Conference: Doha, Qatar. 100. Hopgood, D., Why Improve Hydrate Predictions for Deepwater Black Oil?, in OTC 2001. 2001, Offshore Technology Conference: Houston, Texas. 101. MacDonald, A., et al., Field Application of Combined Kinetic Hydrate and Corrosion Inhibitors in the Southern North Sea: Case Histories, in SPE Gas Technology Symposium. 2006, Society of Petroleum Engineers: Calgary, Alberta, Canada. 102. Guan, H., The Inhibition of Gas Hydrates and Synergy of the Inhibiting Molecules, in International Oil and Gas Conference and Exhibition in China. 2010, Society of Petroleum Engineers: Beijing, China. 103. E.D., S.a.C.A., Koh, Clathrate Hydrates of Natural Gases. 2007, USA: CRC Press. 104. E.D. Sloan, Fundamental Principles and Applications of Natural Gas Hydrates. Nature, 2003. 426(6964): p. 353-363. 105. Lorenzo, M.D. The Hydra Flow Loop; A Tool For Testing The Hydrates Behaviour in Gas Pipelines. in R & D Seminar 2009. Australian resources research center building Perth, Australia: National research flagship/Commonwealth scientific and industrial research organization (CSIRO). 106. Olsen, S., A. Dugstad, and O. Lunde, pH-Stabilization in the Troll Gas-Condensate Pipelines, in Corrosion 99. 1999, NACE International: San Atonia, Texas. 107. PAEZ, J.E. and R. BLOK, Problems in Hydrates: Mechanisms and Elimination Methods, in SPE Production and Operations Symposium. 2001, Copyright 2001, Society of Petroleum Engineers Inc.: Oklahoma City, Oklahoma. 108. Ramachandran, S., et al., Inhibition of Acid Gas Corrosion in Pipelines using Glycol for Hydrate Inhibition, in CORROSION 2006. 2006, NACE International: San Diego Ca. 109. Ethylene Glycol. June 2011; Available from: http://en.wikipedia.org/wiki/Ethylene_glycol. 110. J.Kvarekval, A. Dugstad, and M.Seiersten, Localized Corrosion on Carbon Steel in Sour Glycolic Solutions, in Corrosion 2010. 2010, NACE International: San Antonio, TX. 111. Kvarekval, J. and A. Dugstad, Pitting Corrosion Mechanisms on Carbon Steel in Sour Glycol Water Mixtures, in CORROSION 2004. 2004, NACE International: New Orleans, La. 112. Gonzalez, J.J., G. Pellegrino, and M.E. Alfonso, Corrosion of Carbon Steels in Monoethylene Glycol, in Corrosion 2000. 2000, NACE International: Orlando, Fl. 113. Skar, J.I. and A.M.K. Halvorsen, Corrosion Control in the Vega Gas-Condensate Pipeline, in Corrosion 2010. 2010, NACE International: San Antonio, TX. 114. Kvarekval, J. and A. Dugstad, Corrosion Mitigation with pH Stabilization in Slightly Sour Gas/Condensate Pipelines, in CORROSION 2006. 2006, NACE International: San Diego Ca. 115. Dugstad, A. and M. Seiersten, pH-stabilisation, a Reliable Method for Corrosion Control of Wet Gas Pipelines, in SPE International Symposium on Oilfield Corrosion. 2004, Society of Petroleum Engineers: Aberdeen, United Kingdom. 116. Geir Watterud, M.S., Jens-Petter Andreassen. Iron Carbonate in MEG/Water mixtures. in International Oil Field Chemistry Symposium. 2009. Geilo, Norway. 117. Tobiassen, P. and A.E. Pedersen, Experience Feedback on the Use of a Carbon Steel Subsea Pipeline For A High Pressure, Sweet Service Gas Field, in Corrosion 2004. 2004, NACE International: New Orleans, Louisiana 118. Seiersten, M., et al., Development of a Simulator for Ethylene Glycol Loops Based on Solution Thermodynamics and Particle Formation Kinetics, in Corrosion 2010. 2010, NACE International: San Antonio, TX. 119. Sandengen, K., B. Kaasa, and T. Østvold, pH Measurements in Monoethylene Glycol (MEG) + Water Solutions. Industrial & Engineering Chemistry Research, 2007. 46(14): p. 4734-4739. 120. T.berntsen, M.S.a.T.H., CO2 Corrosion of Carbon Steel at Lower Temperatures in the european corrosion congress (EUROCORR). 2008: Edinburg, Uk,. p. 10. 121. Olsen, S., Corrosion Control by Inhibition, Environmental Aspects, and pH Control: Part II: Corrosion Control by pH Stabilization, in Corrosion 2006. 2006, NACE International: San Diego Ca. 122. Halvorsen, A.M.K., et al., The Reletionship Between Internal Corrosion Control Method, scale Contol and MEG Handling of a Multiphase Carbon Steel Pipeline Carrying Wet Gas with CO2 and Acetic Acid, in Corrosion 2007. 2007, NACE International: Nashville, Tennessee. 123. Hagerup, O. and S. Olsen, Corrosion Control by pH Stabilizer, Materials and Corrosion Monitoring in 160 km Multiphase Offshore Pipeline, in Corrosion 2003. 2003, NACE International: San Diego Ca. 124. Kvarekval, J. and A. Dugstad, Pitting Corrosion in CO2/H2S Containing Glycol Solutions under Flowing Conditions, in Corrosion 2005. 2005, NACE International: Houston, Tx. 125. N.Hackerman, E.S.S.a., NACE Basic Corrosion Course. 1970, NACE: Houston, Texas. 126. Vuorinen, E., E. Kálmán, and W. Focke, Introduction to Vapour Phase Corrosion Inhibitors in Metal Packaging. Surface Engineering, 2004. 20(4): p. 281-284. 127. B.Sanyal, Organic Compounds as Corrosion Inhibitors in Different Environments -A Review. Progress in Organic Compounds as Corrosion 1981. 9(2): p. 165-236. 128. E.Hamner, N., ed. Scope and Importance of Inhibitor Technology. Corrosion Inhibitors, ed. N. C.C. 1973, NACE: Houston, Texas. 1-6. 129. Rostami, A., Review and Evaluation of Corrosion Inhibitors Used in Well Stimulation, in SPE International Symposium on Oilfield Chemistry. 2009, Society of Petroleum Engineers: The Woodlands. Texas. 130. Crouse, M., et al., Evaluation of Potassium Permanganate (KMnO4) as a Green Corrosion Inhibitor/Sealant for Anodized Al 2024 and Al 6061 at Different pH Values, in Corrosion 2002. 2002, NACE International: Denver Co. 131. Okamoto, G., et al., Effect of Organic Inhibitors on the Polarization Characteristics of Mild Steel in Acid Solution. Corrosion Science, 1962. 2(1): p. 21-27. 132. jr, R.l.O., Theoretical Aspects of Corrosion Inhibitors and Inhibition, in Corrosion Inhibitors, N. C.C., Editor. 1981, NACE: Houston Texas. p. 7-27. 133. Meakins, R.J., Alkyl Quaternary Ammonium Compounds as Inhibitors of the Acid Corrosion of Steel. Journal of Applied Chemistry, 1963. 13(8): p. 339-345. 134. Campbell, S. and V. Jovancicevic, Corrosion Inhibitor Film Formation Studied by ATR-FTIR, in Corrosion 99. 1999, NACE International: San Antonio, Tx. 135. Hellberg, P.-E., Environmentally Acceptable Polymeric Corrosion Inhibitors, in SPE International Symposium on Oilfield Chemistry. 2011: The Woodlands, Texas, USA. 136. Mackenzie, C.D., et al., Development of a New Corrosion Management Tool - Inhibitor Micelle Presence as an Indicator of Optimum Dose, in SPE International Conference on Oilfield Corrosion, SPE, Editor. 2010: Aberdeen, UK. 137. Durnie W., D.M.R., Jefferson A., and Kinsella B., Development of a Structure-Activity Relationship for Oil Field Corrosion Inhibitor. The Electrochemical Society, 1999. 146(5): p. 1751-1756. 138. De Marco, R., et al., Persistence of Carbon Dioxide Corrosion Inhibitors. Corrosion, 2002. 58(4): p. 354-363. 139. Vijayalakshmi, P.R. and R. Rajalakshmi, Inhibition of Mild Steel Corrosion Using Aqueous Extract of Cocos nucifera L. Peduncle in Acidic Solutions and Their Adsorption Characteristics, in Corrosion 2013. 2013: Orlando, Florida. 140. Leelavathi, S. and R. Rajalakshmi, Mundulea Sericea Leaves as a Corrosion Inhibitor for Mild Steel in Acidic Solution, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 141. Nalini, D. and R. Rajalakshmi, Inhibition of Mild Steel Corrosion in the Presence of p-Nitrophenyl-2-Imidazoline, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 142. Durnie, W.H., et al., A Study of the Adsorption Properties of Commercial Carbon Dioxide Corrosion Inhibitor Formulations. Journal of Applied Electrochemistry, 2001. 31(11): p. 1221-1226. 143. Gibson, D.H., The Organometallic Chemistry of Carbon Dioxide. Chemical Reviews, 1996. 96(6): p. 2063-2096. 144. N.Hackermann, R.M.H., and R.R.Annand, Corrosion, 1962. 18. 145. Wang D., L.S., Ying Y.,Wang M, Xiao He and Chen Z., Theoretical and Experimental Studies of Structure and Inhibition Efficiency of Iimidazoline Derivatives Corrosion Science, 1999. 41: p. 1911-1919. 146. N.Hackerman, K.A.a., Effect of Molecular Size on Inhibition of Dimethylpolymethylene Ammonium Chloride. Electrochemical Society, 1969. 116(5). 147. Frenier, W.W. and D.G. Hill, Green Inhibitors - Development and Applications for Aqueous Systems, in Corrosion 2004. 2004, NACE International: New Orleans, La. 148. Taj, S., R.W. Revie, and S. Papavinasam, Development of Green Inhibitors for Oil and Gas Applications, in Corrosion 2006. 2006, NACE International: San Diego Ca. 149. Taj, S., et al., Some Natural Products As Green Corrosion Inhibitors, in Corrosion 2007. 2007, NACE International: Nashville, Tennessee. 150. E.Schaschl, Method for Evaluation and Testing of Corrosion Inhibitors. Corrosion Inhibitors, ed. C.C. Nathan. 1973, Houston, Texas: NACE. 28-41. 151. Bregman, J.I., Corrosion Inhibitors. 1963, New York: Macmillan company. 152. Bowman, J.A.K.a.C.W., ed. The Chemistry of Corrosion Inhibitors used in Oil Production,. 1984, UK Corrosion: London. 153. Free, M.L., W. Wang, and D.Y. Ryu, Prediction of Corrosion Inhibition Using Surfactants. Corrosion, 2004. 60(09). 154. Mansfeld, F., S.L. Jeanjaquet, and M.W. Kendig, An Electrochemical Impedance Spectroscopy Study of Reactions at the Metal/Coating Interface. Corrosion Science, 1986. 26(9): p. 735-742. 155. Akbar, A., Understanding the Interactions Between Corrosion Scales and Inhibitor Films in Flow conditions, in School of Mechanical Engineering. 2013, University of Leeds: University of Leeds. 156. Wong, J.E. and N. Park, Effect of Corrosion Inhibitor Active Components on the Growth of Iron Carbonate Scale under CO2 conditions, in Corrosion 2008. 2008, NACE International: New Orleans, Louisiana. 157. Wong, J.E. and N. Park, Further Investigation On The Effect Of Corrosion Inhibitor Actives On The Formation Of Iron Carbonate On Carbon Steel, in Corrosion 2009. 2009, NACE International: Atlanta, Georgia. 158. Tsui, K. and J.E. Wong, Effect Of Corrosion Inhibitor Active Components On Corrosion Inhibition In A Sweet Environment, in Corrosion 2010. 2010, NACE International: San Atonia, Texas. 159. Bikkina, C., et al., Development of MEG Regeneration Unit Compatible Corrosion Inhibitor for Wet Gas Systems, in SPE Asia Pacific Oil and Gas Conference and Exhibition. 2012, Society of Petroleum Engineers: Perth, Australia. 160. Olsen, S., et al., CO2 Corrosion Prediction Model - Basic Principles, in CORROSION 2005. 2005, NACE International: Houston, Tx. 161. Ashton, J.J.B.C. The Effect of Temperature on Conductivity Measurement. 2013; Available from: http://www.camlabworld.com/originalimages/sitefiles/Tech_papers/TempCondMeas.pdf. 162. Bevilacqua, D.M.G.a.A.C. Cation Conductivity Temperature Compensation in International Water Conference,. 1997. Pittsburgh, PA,. 163. Chen, T.-Y., A Transient Technique to Determine Solution Resistance for Corrosion Rate Measurements in Low-Conductivity Solutions, in Corrosion96. 1996, NACE International: Denver , Co. 164. Waxman, M.H. and E.C. Thomas, Electrical Conductivities in Shaly Sands-I. The Relation Between Hydrocarbon Saturation and Resistivity Index; II. The Temperature Coefficient Of Electrical Conductivity. Journal of Petroleum Technology, 1974. 26(2): p. 213-225. 165. Tanupabrungsun, T., B. Brown, and S. Nesic, Effect of pH on CO2 Corrosion of Mild Steel at Elevated Temperatures, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 166. Mishra, B., et al., Development of a Predictive Model for Activation-Controlled Corrosion of Steel in Solutions Containing Carbon Dioxide. Corrosion, 1997. 53(11). 167. Al-Fozan, A.U.M.a.S.A. Pitting Behaviour of Type 316L S.S in Arabian Gulf Seawater. 1992; Available from: http://www.swcc.gov.sa/files%5Cassets%5CResearch%5CTechnical%20Papers%5CCorrosion/PITTING%20BEHAVIOUR%20OF%20TYPE%20316L%20S.S%20INARABIAN%20GULF%20SEAWATER. 168. Azghandi, M., et al., Corrosion Inhibitive Evaluation of an Environmentally Friendly Water-Base Acrylic Terpolymer on Mild Steel in Hydrochloric Acid Media. Metallurgical and Materials Transactions A, 2013. 44(12): p. 5493-5504. 169. R.H.Petrucci, W.S.H., G.E.Herring and J.Madura, General Chemistry Principles & Modern Applications. 2006, New Jersey Prentice Hall. 170. L.Pacheco, J., F.C. Ibrahim, and R. J.Franco, Testing Requirements of Corrosion Inhibitor Qualification for Pipeline Applications, in Corrosion 2010. NACE International: San Antonio, TX. 171. Mok, W.Y., et al., Control of Localized Corrosion using Green Corrosion Inhibitors, in Corrosion 2005. 2005, NACE International: Houston Texas. 172. Frenier, W.W., F.B. Growcock, and V.R. Lopp, Mechanisms of Corrosion Inhibitors Used in Acidizing Wells. SPE Production Engineering, 1988. 3(4): p. 584-590. 173. Hu, X., I.M. Ismail, and A. Neville, Investigation of Pitting Corrosion and Inhibition in Sweet Conditions, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 174. Jenkins, A., Performance of High-Temperature, Biodegradable Corrosion Inhibitors, in Corrosion 2011. 2011, NACE International: Houston, Texas. 175. Magana-Zavala, C.R., et al., Electrochemical Impedance Spectroscopy (EIS) Modelling of Different Behaviours of Ni and Ni Oxide Thin Films for Corrosion Prevention in Sour Media. Anti-Corrosion Methods and Materials, 2010. 57(3): p. 118-125. 176. Castaneda, H., E. Sosa, and M.A. Espinosa-Medina, Film Properties and Stability Influence on Impedance Distribution During the Dissolution Process of Low-carbon Steel Exposed to Modified Alkaline Sour Environment. Corrosion Science, 2009. 51(4): p. 799-806. 177. Lopez, H.C., et al., Film Stability for API 5L X-52 Line Pipe Steel in CO2 (aq) and Cl (aq) Solutions in Presence of Amine Based Inhibitor under Hydrodynamic Conditions, in Corrosion 2004. 2004, NACE International: New Orleans, Louisiana. 178. Duval, S., R. Sauvant-Moynot, and F. Ropital, EIS: A Powerful Tool for In Situ Monitoring Coating Performance, in Corrosion 2003. 2003, NACE International: San Diego, Ca. 179. Wang, H., et al., Characterization of Inhibitor and Corrosion Product Film Using Electrochemical Impedance Spectroscopy (EIS), in Corrosion 2001. 2001, NACE International: Houston, Texas. 180. Lillard, R.S., et al., Using Local Electrochemical Impedance Spectroscopy to Examine Coating Failure. Corrosion, 1995. 51(04). 181. Ruedisueli, R.L., A. Sheetz, and A. Field, Paint Coating Electrical Resistance and Performance in Service Environments, in Corrosion 2006. 2006, NACE International: San Diego, Ca. 182. Torres-Islas, A., et al., Corrosion Inhibition Efficiency Study in a Microalloyed Steel for Sour Service at 50 degrees C. Journal of Applied Electrochemistry, 2010. 40(8): p. 1483-1491. 183. Mansfeld, F., et al., Analysis of Electrochemical Impedance and Noise Data for Polymer Coated Metals. Corrosion Science, 1997. 39(2): p. 255-279. 184. Esih I., S.T.a.P.Z. Inhibition of Mild Steel Corrosion in CO2-Saturated Chloride Solutions by Acylated Polyamine Salts. in Proceedings of the 8th European Symposium on Corrosion Inhibitors (8 SEIC). 1995. Ann, Univ. Ferrara, N.S. 185. Halvorsen, E.N., et al., Qualification of Scale Inhibitors for Subsea Tiebacks With MEG Injection, in SPE International Symposium on Oilfield Chemistry. 2009, Society of Petroleum Engineers: The Woodlands. Texas. 186. Nesic, S. and K.-L.J. Lee, A Mechanistic Model for Carbon Dioxide Corrosion of Mild Steel in the Presence of Protective Iron Carbonate FilmsPart 3: Film Growth Model. Corrosion, 2003. 59(07). 187. Nesic, S., et al., A Mechanistic Model for Carbon Dioxide Corrosion of Mild Steel in the Presence of Protective Iron Carbonate Films - Part 2: A Numerical Experiment. Corrosion, 2003. 59(6): p. 489-497. 188. Llongueras, J.G., et al., Mechanism of FeCO3 Formation on API X70 Pipeline Steel in Brine Solutions Containing CO2, in Corrosion 2005. 2005, NACE International: Houston, Texas. 189. Nordsveen, M., et al., A mechanistic model for carbon dioxide corrosion of mild steel in the presence of protective iron carbonate films - Part 1: Theory and verification. Corrosion, 2003. 59(5): p. 443-456. 190. Han, J., et al., Electrochemical Investigation of Localized CO2 Corrosion on Mild Steel, in Corrosion 2007. 2007, NACE International: Nashville, Tennessee. 191. Hitoshi Shindo, a.M.K., Stabilities of Crystal Faces of Aragonite (CaCO3) Compared by Atomic Force Microscopic Observation of Facet Formation Processes in Aqueous Acetic acid. Physical Chemistry Chemical Physics, 2005. 7(4): p. 691-6. 192. Ahmad, Z., Principles of Corrosion Engineering and Corrosion Control. Materials & Mechanical. 2006: Butterworth-Heinemann. 1-672. 193. Hong, T., et al., EIS Study of Corrosion Product Film in Pipelines, in Corrosion 2000. NACE International: Orlando, Florida. 194. Gulbrandsen, E. and J.H. Morard, Study of the Possible Mechanisms of Steel Passivation in CO2 Corrosion, in Corrosion 99. 1999, NACE International: San Antonio, Tx. 195. Riemenschneider, W. and H.M. Bolt, Esters, Organic, in Ullmann's Encyclopedia of Industrial Chemistry. 2000, Wiley-VCH Verlag GmbH & Co. KGaA. 196. Ismail, I.M., Inhibition of Pitting on Carbon Steel, in School of Mechanical Engineering. 2011, University of Leeds: University of Leeds. 197. Alink, B.A., et al., Mechanism of CO2 Corrosion Inhibition by Phosphate Esters, in Corrosion99. 1999, NACE International: San Atonia, Texas. 198. Sun, W., K. Chokshi, and S. Nesic, Iron Carbonate Scale Growth and the Effect of Inhibition in CO2 Corrosion of Mild Steel. 2005, NACE International. 199. Nyborg, R., et al., Effect of Steel Microstructure and Composition on Inhibition of CO2 Corrosion, in Corrosion 2000. 2000, NACE International: Orlando, Fl. 200. Kvarekval, J., S. Skjerve, and S. Olsen, The Effect of O2 on CO2 Corrosion in pH Stabilized Gas/Condensate Pipelines, in Corrosion 2005. 2005, NACE International: Houston, Tx. 201. Lu, H., A.T. Kan, and M.B. Tomson, Effects of Monoethylene Glycol on Carbonate Equilibrium and Calcite Solubility in Gas/Monoethylene Glycol/Water/Salt Mixed Systems, in SPE International Symposium on Oilfield Chemistry. 2009, Society of Petroleum Engineers: The Woodlands. Texas. 202. Vuppu, A.K. and W.P. Jepscm, Study Of Sweet Corrosion In Horizontal Multiphase, Carbon Steel Pipelines, in OTC 1994, Offshore Technology Conference: Houston, Texas. 203. Nordsveen, M., S.N.R. Nyborg, and A. Stangeland, A Mechanistic Model for Carbon Dioxide Corrosion of Mild Steel in the Presence of Protective Iron Carbonate FilmsPart 1: Theory and Verification. Corrosion, 2003. 59(05). 204. Han, J., B.N. Brown, and S. Nesic, Investigation of the Galvanic Mechanism for Localized Carbon Dioxide Corrosion Propagation Using the Artificial Pit Technique. Corrosion, 2010. 66(9). 205. Berntsen, T., M. Seiersten, and T. Hemmingsen, Effect of FeCO3 Supersaturation And Carbide Exposure On the CO2 Corrosion Rate of Carbon Steel, in Corrosion 2011. 2011, NACE International: Houston, Texas."]},{"key":"dc:type","label":"Dc Type","values":["Thesis"]},{"key":"dc:type.qualificationlevel","label":"Dc Type Qualificationlevel","values":["doctoral"]},{"key":"dc:type.qualificationname","label":"Dc Type Qualificationname","values":["Ph.D"]}]},{"id":"language_rights","label":"Language and Rights","entries":[{"key":"dc:language.dcterms_iso639_2","label":"Language (ISO 639-2)","values":["eng"]}]},{"id":"identifiers","label":"Identifiers","entries":[{"key":"dc:identifier","label":"Identifier","values":["uk.bl.ethos.635382"]},{"key":"dc:identifier.uri","label":"Identifier URI","values":["https://etheses.whiterose.ac.uk/id/eprint/7329/1/Ikechukwu%20C.%20Ivonye%20Thesis.pdf"]}]},{"id":"additional","label":"Additional Metadata","entries":[{"key":"dc:description.abstract","label":"Abstract","values":["Carbon steel pipelines are employed in the oil and gas industry for long distance multiphase transportation. The integrity of these pipelines is critical to oil and gas production. Transportation of wet natural gas using carbon steel pipelines from source to processing plant may lead to corrosion, hydrate formation and even scale formation. To prevent hydrate formation MonoEthylene Glycol (MEG) is pumped through the pipeline. Corrosion inhibitors and other corrosion prevention methods may be employed to reduce corrosion to manageable and acceptable levels. In this study the corrosion inhibition properties of MEG were investigated at both low and high temperature conditions. The reduction of carbon steel X65 corrosion in the presence of MEG alone and 1% NaCl alone at low temperature of 20°C was in line with previous studies. At high temperature of 80°C, the corrosion rate of the carbon steel in the presence of MEG tends to increase. Thus the reduction of the corrosion rate of carbon steel in the presence of MEG can be underestimated. The increase in the corrosion rate of carbon steel in the presence of MEG at high temperature led to the search for the mechanism by which MEG reduces corrosion. The adsorption process was studied using Fourier transform infra-red spectroscopy (FTIR). Further determination of the adsorption isotherm properties and behaviour of MEG on the corrosion of carbon steel was recorded through experimentation. The results were used to determine the type of adsorption that occurs in the presence of MEG. The corrosion rate of carbon steel in the presence of MEG is improved by deployment of chemical inhibitors to reach a minimal acceptable rate. This study investigated the use of two types of commercially-available inhibitors green (inhibitor 2) and non-green inhibitor (inhibitor 1) for reduction of the corrosion rate. The effects of the two inhibitors alone on the corrosion of carbon steel at both high and low temperatures were first examined. This enabled an assessment of the inhibitor in the presence of MEG. A combination of the MEG and inhibitor was tested at both low and high concentrations. The influence on MEG on the inhibitor performance was determined. Conditions necessary for the formation of protective iron carbonate were determined and used for pre-corrosion. The influence of iron carbonate on the corrosion of carbon steel was determined. Pre-corroded carbon steel was used to assess the influence of MEG in the presence of iron carbonate. Further test on the pre-corroded carbon steel in the presence of MEG and inhibitor was performed to assess the influence of the inhibitor and MEG on iron carbonate scale."]},{"key":"dc:format","label":"Dc Format","values":["text"]},{"key":"dcterms:accessrights","label":"Dcterms Accessrights","values":["public"]},{"key":"dc:title","label":"Title","values":["Corrosion processes and mechanisms in the presence of MonoEthylene Glycol (MEG)"]}]}],"canonical_facts":{"dc:contributor.advisor":["Neville, Anne","Wang, Chun"],"dc:creator":["Ivonye, Ikechukwu C."],"dc:date":["2014-07"],"dc:date.issued":["2014-07"],"dc:description.abstract":["Carbon steel pipelines are employed in the oil and gas industry for long distance multiphase transportation. The integrity of these pipelines is critical to oil and gas production. Transportation of wet natural gas using carbon steel pipelines from source to processing plant may lead to corrosion, hydrate formation and even scale formation. To prevent hydrate formation MonoEthylene Glycol (MEG) is pumped through the pipeline. Corrosion inhibitors and other corrosion prevention methods may be employed to reduce corrosion to manageable and acceptable levels. In this study the corrosion inhibition properties of MEG were investigated at both low and high temperature conditions. The reduction of carbon steel X65 corrosion in the presence of MEG alone and 1% NaCl alone at low temperature of 20°C was in line with previous studies. At high temperature of 80°C, the corrosion rate of the carbon steel in the presence of MEG tends to increase. Thus the reduction of the corrosion rate of carbon steel in the presence of MEG can be underestimated. The increase in the corrosion rate of carbon steel in the presence of MEG at high temperature led to the search for the mechanism by which MEG reduces corrosion. The adsorption process was studied using Fourier transform infra-red spectroscopy (FTIR). Further determination of the adsorption isotherm properties and behaviour of MEG on the corrosion of carbon steel was recorded through experimentation. The results were used to determine the type of adsorption that occurs in the presence of MEG. The corrosion rate of carbon steel in the presence of MEG is improved by deployment of chemical inhibitors to reach a minimal acceptable rate. This study investigated the use of two types of commercially-available inhibitors green (inhibitor 2) and non-green inhibitor (inhibitor 1) for reduction of the corrosion rate. The effects of the two inhibitors alone on the corrosion of carbon steel at both high and low temperatures were first examined. This enabled an assessment of the inhibitor in the presence of MEG. A combination of the MEG and inhibitor was tested at both low and high concentrations. The influence on MEG on the inhibitor performance was determined. Conditions necessary for the formation of protective iron carbonate were determined and used for pre-corrosion. The influence of iron carbonate on the corrosion of carbon steel was determined. Pre-corroded carbon steel was used to assess the influence of MEG in the presence of iron carbonate. Further test on the pre-corroded carbon steel in the presence of MEG and inhibitor was performed to assess the influence of the inhibitor and MEG on iron carbonate scale."],"dc:format":["text"],"dc:identifier":["uk.bl.ethos.635382"],"dc:identifier.uri":["https://etheses.whiterose.ac.uk/id/eprint/7329/1/Ikechukwu%20C.%20Ivonye%20Thesis.pdf"],"dc:language.dcterms_iso639_2":["eng"],"dc:publisher.commercial":["University of Leeds"],"dc:publisher.department":["School of Mechanical Engineering (Leeds)","Institute of Engineering Thermofluids, Surfaces & Interfaces (iETSI) (Leeds)"],"dc:publisher.institution":["University of Leeds"],"dc:relation.isreferencedby":["https://etheses.whiterose.ac.uk/id/eprint/7329/"],"dc:relation.references":["1. Christof, R. BP Energy Outlook 2035 2014 [cited 2014 21/03/2014]; 4th edition:[Available from: http://www.bp.com/en/global/corporate/about-bp/energy-economics/energy-outlook.html?gclid=CMWg5YyXpL0CFS7MtAodiVIAKg. 2. Brustad, S., K.-P. Løken, and J.G. Waalmann, Hydrate Prevention using MEG instead of MeOH: Impact of experience from major Norwegian developments on technology selection for injection and recovery of MEG, in Offshore Technology Conference. 2005: Houston, Texas. 3. L.Fosb, P., K. Thomsen, and E. H.Stenby, Improving Mechanistic CO2 Corrosion Models in CORROSION 2009. 2009, NACE International: Atlanta, GA. 4. Revie, R.W., Uhlig H. Herbert, Corrosion and Corrosion Control : An Introduction to Corrosion Science and Engineering. 4th ed. 2008, Hoboken, N.J.: J. Wiley. 5. G.H.Koch, M.P.H.B., N.G.Thompson,Y.P.Virmani, and J.H.Payer, Corrosion Cost and Preventon Strategies in the United States,. 2002, Federal highway administration, U.S. Department of Transportation: McLean VA. 6. Papavinasam, S., Corrosion Control in the Oil and Gas Industry. 2014, London, UK: Elsevier Inc. 7. Utility Board (ERCB) 91-G Report 2007, Alberta Energy Regulator (AER): 250-5th street SW, Calgary, Alberta, Canada,. 8. Wang, C., Erosion-Corrosion Mitigation Using Chemicals, in School of Mechanical Engineering. 2007: University of Leeds. 9. Barker, R.J., Erosion-Corrosion of Carbon Steel Pipework on an Offshore Oil and Gas facility, in School of Mechanical Engineering. 2012, University of Leeds: University of Leeds. 10. R.A.Buchanan, E.E.S.a., Fundamentals of Electrochemical Corrosion. 2000, Ohio: ASM International. 11. Tait, W.S., ed. An Introduction to Electrochemical Corrosion Testing for Practicing Engineers and Scientists. 1994, Racine, WI: Pair O Docs Publications. 12. Ren, C.Q., et al., Corrosion Behavior of Oil Tube Steel in Simulant Solution with Hydrogen Sulfide and Carbon Dioxide. Materials Chemistry and Physics, 2005. 93(2-3): p. 305-309. 13. ; Available from: http://chemwiki.ucdavis.edu/Analytical_Chemistry/Analytical_Chemistry_2.0/11_Electrochemical_Methods/11B_Potentiometric_Methods. 14. Sastri, V.S., Corrosion Prevention and Protection : Practical Solutions. 2007, Chichester: Wiley. 15. Revie, R.W., Uhlig's Corrosion Handbook. 2nd ed. 2000, New York: Wiley. 16. Thomas, J., The Mechanism of Corrosion Prevention by Inhibitors, in Corrosion Control, L.L.Shreir, Editor. 1979, Newnes-Butterworths: Uk. 17. Sastri, V.S., Corrosion Inhibitors : Principles and Applications 1998, Chichester ; New York :: Wiley. 18. Denzine, A.F. and M.S. Reading, A Critical Comparison of Corrosion Monitoring Techniques used in Industrial applications, in Corrosion97. 1997, NACE International: New Orleans, LA. 19. Scully, J.R., The Polarization Resistance Method for Determination of Instantaneous Corrosion Rates: A Review, in CORROSION 98. 1998, NACE International: San Diego Ca. 20. Scully, J.R., Polarization Resistance Method for Determination of Instantaneous Corrosion Rates. Corrosion, 2000. 56(2): p. 199-218. 21. Nesic, S., Key Issues Related to Modelling of Internal Corrosion of Oil and Gas Pipelines - A Review. Corrosion Science, 2007. 49(12): p. 4308-4338. 22. Sun, W., S. Nesic, and R.C. Woollam, The Effect of Temperature and Ionic Strength on Iron Carbonate (FeCO3) Solubility limit. Corrosion Science, 2009. 51(6): p. 1273-1276. 23. Wang, X., et al., Comprehensive Study of the Hydration and Dehydration Reactions of Carbon Dioxide in Aqueous Solution. The Journal of Physical Chemistry A, 2009. 114(4): p. 1734-1740. 24. Alberty, R., Physical Chemistry. 1983: John Wiley and Sons 25. Bruno, J., The Influence of Dissolved Carbon dioxide on Trace Metal Speciation in Seawater. Marine Chemistry, 1990. 30(0): p. 231-240. 26. Palmer, D.A. and R. Van Eldik, The Chemistry of Metal Carbonato and Carbon dioxide Complexes. Chemical Reviews, 1983. 83(6): p. 651-731. 27. Nesic, S., et al., An Open Source Mechanistic Model for CO2 /H2S Corrosion of Carbon Steel, in CORROSION 2009. 2009, NACE International: Atlanta, GA. 28. Schmitt, G. and M. Horstemeier, Fundamental Aspects of CO2 Metal Loss Corrosion - Part II: Influence of Different Parameters on CO2 Corrosion Mechanisms, in Corrosion 2006. 2006, NACE International: San Diego Ca. 29. J. O'M. Bockris, N.B., F. Gutmann, An Introduction to Electrochemical Science 1974, London Wykeham Publications. 30. J.O.M. Bockris, D.D., A.R. Despic, , The Electrode Kinetics of the Deposition and Dissolution of iron. Electrochemica acta, 1965. 4: p. 325-361. 31. J.O.M. Bockris, D.M.D., Electro-Chemical Science. 1972, Taylor and Francis: London. 32. Nesic, S., J. Postlethwaite, and S. Olsen, An Electrochemical Model for Prediction of Corrosion of Mild Steel in Aqueous Carbon Dioxide Solutions. Corrosion, 1996. 52(04). 33. Dugstad, A., Mechanism of Protective Film Formation During CO2 Corrosion of Carbon Steel, in CORROSION 98. 1998, NACE International: San Diego Ca. 34. Nyborg, R., Overview of CO2 Corrosion Models for Wells and Pipelines, in CORROSION 2002. 2002, NACE International: Denver, Co. 35. Kermani, M.B. and A. Morshed, Carbon Dioxide Corrosion in Oil and Gas ProductionA Compendium. Corrosion, 2003. 59(08). 36. de Waard, C. and D.E. Milliams, Carbonic Acid Corrosion of Steel. Corrosion, 1975. 31(5): p. 177-181. 37. Hurlen, T., Corrosion of Iron-Effect of pH and Ferrous Ion Activity Acta Chemica Scandinavica, 1960. 14(7): p. 1555-1563. 38. L.G.S. Gray, B.G.A., M.J. Danysh, P.G. Tremaine, , Mechanism of Carbon Steel Corrosion in Brines Containing Dissolved Carbon Dioxide at pH 4, in Corrosion89. 1989, NACE: Houston Tx. 39. L.G.S. Gray, B.G.A., M.J. Danysh, P.R. Tremaine, , Effect of pH and Temperature on the Mechanism of Carbon Steel Corrosion by Aqueous Carbon dioxide, in NACE International. 1990, NACE: Houston Tx. 40. Nesic, S., et al., Electrochemical Properties of Iron Dissolution in the Presence of CO2 - Basics Revisited, in CORROSION 96. 1996, NACE International: Denver, Co. 41. Dewaard, C. and D.E. Milliams, CARBONIC-ACID CORROSION OF STEEL. Corrosion, 1975. 31(5): p. 177-181. 42. Schmitt, G. and B. Rothmann, Investigations into Corrosion Mechanism of Unalloyed Steel in Oxygen-Free Carbonic-Acid Solutions .1. Kinetics of Hydrogen Evolution. Werkstoffe Und Korrosion-Materials and Corrosion, 1977. 28(12): p. 816-822. 43. Schmitt, G. and B. Rothmann, Investigations into Corrosion of Mild-Steel in Oxygen-Free Carbon-dioxide Solutions.2. Kinetic of Iron Dissolution. Werkstoffe Und Korrosion-Materials and Corrosion, 1978. 29(2): p. 98-100. 44. Schmitt, G. and B. Rothmann, Corrosion of Unalloyed and Low Alloyed Steels in Carbonic-Acid Solutions. Werkstoffe Und Korrosion-Materials and Corrosion, 1978. 29(4): p. 237-245. 45. Ogundele, G.I. and W.E. White, Some Observations on Corrosion of Carbon-Steel in Aqueous Environments Containing Carbon-dioxide. Corrosion, 1986. 42(2): p. 71-78. 46. Mora-Mendoza, J.L. and S. Turgoose, Influence of Turbulent Flow on the Localized Corrosion Processes of Mild Steel With Inhibited Aqueous CO2 Systems, in CORROSION 2001. 2001, NACE International: Houston, Tx. 47. Postlethwaite, J. and D. Wang, Modeling Aqueous CO2 Corrosion of Iron in Turbulent Pipe Flow, in Corrosion 2001. 2001, NACE International: Houston, Texas. 48. Nesic, S., G.T. Solvi, and J. Enerhaug, Organic Materials Generally are Recognized as Effective Inhibitors of the Corrosion of Many Metals and Alloys. Corrosion, 1995. 51(10). 49. Videm, K. and A.M. Koren, Corrosion, Passivity, and Pitting of Carbon-Steel in Aqueous-Solutions of HCO3 -, CO2, and Cl- Corrosion, 1993. 49(9): p. 746-754. 50. K.Videm, A.D., Corrosion of Carbon Steel in an Aqueous Carbon dioxide Environment. Part 2. Film Formation,. material Performance, 1989. 28: p. 46-50. 51. Ikeda, A., S. Mukai, and M. Ueda, Relationship Between Environmental-factors and Corrosion Product on CO2 Corrosion. Transactions of the Iron and Steel Institute of Japan, 1984. 24(12): p. B401-B401. 52. Ikeda, A., CO2 Corrosion of Iron and Steel in Oil and Gas Production. Journal of the Japan Petroleum Institute, 2002. 45(2): p. 55-69. 53. de Waard, C., U. Lotz, and D.E. Milliams, Predictive Model for CO2 Corrosion Engineering in Wet Natural Gas Pipelines. Corrosion, 1991. 47(12): p. 976-985. 54. Palacios, C.A.a.S., J.R., Characteristics of Corrosion Scales on Steel in a CO2-Saturated NaCl Brine. Corrosion, 1991. 47(2): p. 122-127. 55. Papavinasam, S., A. Doiron, and R.W. Revie, Effect of Surface Layers on the Initiation of Internal Pitting Corrosion in Oil and Gas Pipelines. Corrosion, 2009. 65(10): p. 663-673. 56. Papavinasam, S., A. Doiron, and R.W. Revie, Model to Predict Internal Pitting Corrosion of Oil and Gas Pipelines. Corrosion, 2010. 66(3). 57. Nyborg, R. and A. Dugstad, Understanding and Prediction of Mesa Corrosion Attack, in CORROSION 2003. 2003, NACE International: San Diego Ca. 58. Schmitt, G.A., et al., Understanding Localized CO2 Corrosion of Carbon Steel from Physical Properties of Iron Carbonate Scales, in Corrosion99. 1999, NACE International: San Antonio, Texas. 59. Heuer, J.K. and J.F. Stubbins, An XPS Characterization of FeCO3 Films from CO2 Corrosion. Corrosion Science, 1999. 41(7): p. 1231-1243. 60. John, R.C., et al., SweetCor: An Information System for the Analysis of Corrosion of Steels by Water and Carbon Dioxide, in CORROSION 98. 1998, NACE International: San Diego Ca. 61. Xia, Z., K.C. Chou, and Z. Szklarskasmialowska, Pitting Corrosion of Carbon-Steel in CO2-Containing Nacl Brine. Corrosion, 1989. 45(8): p. 636-642. 62. Farelas, F., B. Brown, and S. Nesic, Iron Carbide and its Influence on the Formation of Protective Iron Carbonate in CO2 Corrosion of Mild Steel, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 63. J-L.Crolet and M.R.Bonis, Alogorithm of the Protectiveness of Corrosion Layers 1-Protectiveness Mechanism and CO2 Corrosion Prediction, in Corrosion 2010. 2010, NACE International: San Antonio, Texas. 64. Crolet, J.L., N. Thevenot, and S. Nesic, Role of Conductive Corrosion Products in the Protectiveness of Corrosion Layers. Corrosion, 1998. 54(03). 65. Crolet, J.L., S. Nesic, and N. Thevenot, Role of Conductive Corrosion Products on the Protectiveness of Corrosion Layers, in CORROSION 96. 1996, NACE International: Denver, Co. 66. De Waard, C., U. lotz, and A. Dugstad, Influence of Liquid Flow Velocity on CO2 Corrosion: A Semi-Emprical Model, in Corrosion 95. 1995, NACE USA. 67. De Waard, C. and U. lotz, Prediction of CO2 Corrosion of Carbon Steel, in Corrosion 93. 1993, NACE: USA. 68. Harris, M.G., M.C.D. Adams, and D.J.D. Garber, Use of a Corrosion Prediction Program as an Engineering Tool, in Corrosion97. 1997, NACE International: New Orleans, LA. 69. Woollam, R.C. and S. Hernandez, Assessment and comparison of CO2 corrosion predicition models, in SPE International Oilfield Corrosion Symposium. 2006: Aberdeen, UK. 70. Hunnik, E.V., B.F.M. Pots, and E.L.J.A. Hendriksen, The Formation of Protective Fe3CO2 Corrosion Product Layers in CO Corrosion, in Corrosion96. 1996, NACE International: Denver, Colorado. 71. Pots, B.F.M., Mechanistic Models for the Prediction of CO2 Corrosion Rates Under Multi-Phase Flow Conditions, in CORROSION. 1995, NACE. 72. Nyborg, R., A. Dugstad, and L. Lunde, Corrosion and Glycol Distribution in a Large Wet-Gas Pipeline. Materials Performance, 1993. 32(9): p. 57-61. 73. Ayello, F.x.o., et al., Determination of Phase Wetting in Oil-Water Pipe Flows in CORROSION 2008. 2008, NACE International: New Orleans LA. 74. M. Wicks, J.P.F.M., Material Performance, 1975. 9. 75. Halvorsen, A.M. and T. Sontvedt, CO2 Corrosion Model for Carbon Steel Including Wall Shear Stress Model for Multiphase Flow and Limits for Production Rate to Avoid Mesa Attack, in CORROSION 99. 1999, NACE International: San Antonio, Tx. 76. Adams, C.D., et al., Computer Modeling to Predict Corrosion Rates in Gas Condensate Wells Containing CO2, in CORROSION 96. 1996, NACE International: Denver, Co. 77. Dugstad, A., M. Seiersten, and R. Nyborg, Flow Assurance of pH Stabilized Wet Gas Pipelines, in CORROSION 2003. 2003, NACE International: San Diego Ca. 78. Sun, W. and S. Nesic, Kinetics of Corrosion Layer Formation: Part 1 - Iron Carbonate Layers in Carbon dioxide Corrosion. Corrosion, 2008. 64(4): p. 334-346. 79. Dugstad, A., Formation of Protective Corrosion Films during CO2 Corrosion of Carbon Steel. Advances in Corrosion Control and Materials in Oil and Gas Production, 1999(26): p. 70-76. 80. J.L.Crolet, S.O., W.Wilhelmsen, Influence of a Layer of Indissolved Cementite on the Rate of the CO2 Corrosion of Carbon steel, in Corrosion94. 1994: Houston, Tx. 81. Seal, S., et al., The Effect of Flow on the Corrosion Product Layer in Presence of Corrosion Inhibitors, in CORROSION 2002. 2002, NACE International: Denver, Co. 82. Wang, H., et al., Why Corrosion Inhibitors Do Not Perform Well in Some Multiphase Conditions: A Mechanistic Study, in Corrosion 2002. 2002, NACE International: Denver, Colorado. 83. Chen, H.J. and W.P. Jepson, Inhibition of Slug Front Corrosion in Multiphase Flow Conditions, in CORROSION 98. 1998, NACE International: San Diego Ca. 84. Al-Hassan, S., et al., Effect of Microstructure on Corrosion of Steels in Aqueous Solutions Containing Carbon Dioxide. Corrosion, 1998. 54(06). 85. Dugstad, A., H. Hemmer, and M. Seiersten, Effect of Steel Microstructure on Corrosion Rate and Protective Iron Carbonate Film Formation. Corrosion, 2001. 57(04). 86. Dugstad, A. and P.-E. Dronen, Efficient Corrosion Control of Gas Condensate Pipelines by pH - Stabilization, in Corrosion 99. 1999, NACE International. 87. Gulbrandsen, E. and J.H. Morard, Why Does Glycol Inhibit CO2 Corrosion?, in CORROSION 98. 1998, NACE International: San Diego Ca. 88. Garsany, Y., D. Pletcher, and B.M. Hedges, The Role of Acetate in CO2 Corrosion of Carbon Steel: Has the Chemistry Been Forgotten?, in Corrosion 2002. 2002, NACE International: Denver, Colorado. 89. Garsany, Y., et al., Quantifying the Acetate-Enhanced Corrosion of Carbon Steel in Oilfield Brines, December 2004. Corrosion, 2004. 60(12). 90. Sun, Y., K. George, and S. Nesic, The Effect of Cl- and Acetic Acid on Localized CO2 Corrosion in Wet Gas Flow, in Corrosion 2003. 2003, NACE International: San Diego Ca. 91. George, K., K.d. Waard, and S. Nesic, Electrochemical Investigation and Modeling of Carbon Dioxide Corrosion of Carbon Steel in the Presence of Acetic Acid. 2004, NACE International. 92. Crolet, J.L., A. Dugstad, and N. Thevenot, Role of Free Acetic Acid on the CO2 Corrosion of Steels, in CORROSION 99. 1999, NACE International: San Antonio, Tx. 93. Gulbrandsen, E. and K. Bilkova, Solution Chemistry Effects on Corrosion of Carbon Steels in Presence of CO2 and Acetic Acid, in Corrosion 2006. 2006, NACE International: San Diego, California. 94. Nafday, O. and S. Nesic, Iron Carbonate Scale Formation and CO2 Corrosion in the Presence of Acetic Acid, in Corrosion 2005. 2005, NACE International: Houston, Texas. 95. Wheeler, P.J., lntroduction to the Troll Project, in OTC 97. 1997, Offshore Technology Conference: Houston, Texas. 96. Rebsdat, S. and D. Mayer, Ethylene Glycol, in Ullmann's Encyclopedia of Industrial Chemistry. 2000, Wiley-VCH Verlag GmbH & Co. KGaA. 97. Rebsdat, S. and D. Mayer, ETHYLENE GLYCOL. Gerhartz, W., Et Al. (Ed.). Ullmann's Encyclopedia of Industrial Chemistry, Fifth Completely Revised Edition, Vol. A 10. Ethanolamines to Fibers, 4. Synthetic Organic. Xv+655p. Vch Publishers, Inc.: New York, New York, USA; Cambridge, England, Uk; Vch Verlagsgesellschaft Mbh: Weinheim, West Germany. Illus. Maps, 1987: p. 101-116. 98. Boxall, J., et al., Predicting When and Where Hydrate Plugs Form in Oil-Dominated Flowlines. SPE Projects, Facilities & Construction, 2009. 4(3): p. pp. 80-86. 99. Elhady, A.A.A., Operating Experiences of DEG and MEG for Hydrate and Dew Point Control in Gas Production Offshore Mediterranean, in International Petroleum Technology Conference. 2005, International Petroleum Technology Conference: Doha, Qatar. 100. Hopgood, D., Why Improve Hydrate Predictions for Deepwater Black Oil?, in OTC 2001. 2001, Offshore Technology Conference: Houston, Texas. 101. MacDonald, A., et al., Field Application of Combined Kinetic Hydrate and Corrosion Inhibitors in the Southern North Sea: Case Histories, in SPE Gas Technology Symposium. 2006, Society of Petroleum Engineers: Calgary, Alberta, Canada. 102. Guan, H., The Inhibition of Gas Hydrates and Synergy of the Inhibiting Molecules, in International Oil and Gas Conference and Exhibition in China. 2010, Society of Petroleum Engineers: Beijing, China. 103. E.D., S.a.C.A., Koh, Clathrate Hydrates of Natural Gases. 2007, USA: CRC Press. 104. E.D. Sloan, Fundamental Principles and Applications of Natural Gas Hydrates. Nature, 2003. 426(6964): p. 353-363. 105. Lorenzo, M.D. The Hydra Flow Loop; A Tool For Testing The Hydrates Behaviour in Gas Pipelines. in R & D Seminar 2009. Australian resources research center building Perth, Australia: National research flagship/Commonwealth scientific and industrial research organization (CSIRO). 106. Olsen, S., A. Dugstad, and O. Lunde, pH-Stabilization in the Troll Gas-Condensate Pipelines, in Corrosion 99. 1999, NACE International: San Atonia, Texas. 107. PAEZ, J.E. and R. BLOK, Problems in Hydrates: Mechanisms and Elimination Methods, in SPE Production and Operations Symposium. 2001, Copyright 2001, Society of Petroleum Engineers Inc.: Oklahoma City, Oklahoma. 108. Ramachandran, S., et al., Inhibition of Acid Gas Corrosion in Pipelines using Glycol for Hydrate Inhibition, in CORROSION 2006. 2006, NACE International: San Diego Ca. 109. Ethylene Glycol. June 2011; Available from: http://en.wikipedia.org/wiki/Ethylene_glycol. 110. J.Kvarekval, A. Dugstad, and M.Seiersten, Localized Corrosion on Carbon Steel in Sour Glycolic Solutions, in Corrosion 2010. 2010, NACE International: San Antonio, TX. 111. Kvarekval, J. and A. Dugstad, Pitting Corrosion Mechanisms on Carbon Steel in Sour Glycol Water Mixtures, in CORROSION 2004. 2004, NACE International: New Orleans, La. 112. Gonzalez, J.J., G. Pellegrino, and M.E. Alfonso, Corrosion of Carbon Steels in Monoethylene Glycol, in Corrosion 2000. 2000, NACE International: Orlando, Fl. 113. Skar, J.I. and A.M.K. Halvorsen, Corrosion Control in the Vega Gas-Condensate Pipeline, in Corrosion 2010. 2010, NACE International: San Antonio, TX. 114. Kvarekval, J. and A. Dugstad, Corrosion Mitigation with pH Stabilization in Slightly Sour Gas/Condensate Pipelines, in CORROSION 2006. 2006, NACE International: San Diego Ca. 115. Dugstad, A. and M. Seiersten, pH-stabilisation, a Reliable Method for Corrosion Control of Wet Gas Pipelines, in SPE International Symposium on Oilfield Corrosion. 2004, Society of Petroleum Engineers: Aberdeen, United Kingdom. 116. Geir Watterud, M.S., Jens-Petter Andreassen. Iron Carbonate in MEG/Water mixtures. in International Oil Field Chemistry Symposium. 2009. Geilo, Norway. 117. Tobiassen, P. and A.E. Pedersen, Experience Feedback on the Use of a Carbon Steel Subsea Pipeline For A High Pressure, Sweet Service Gas Field, in Corrosion 2004. 2004, NACE International: New Orleans, Louisiana 118. Seiersten, M., et al., Development of a Simulator for Ethylene Glycol Loops Based on Solution Thermodynamics and Particle Formation Kinetics, in Corrosion 2010. 2010, NACE International: San Antonio, TX. 119. Sandengen, K., B. Kaasa, and T. Østvold, pH Measurements in Monoethylene Glycol (MEG) + Water Solutions. Industrial & Engineering Chemistry Research, 2007. 46(14): p. 4734-4739. 120. T.berntsen, M.S.a.T.H., CO2 Corrosion of Carbon Steel at Lower Temperatures in the european corrosion congress (EUROCORR). 2008: Edinburg, Uk,. p. 10. 121. Olsen, S., Corrosion Control by Inhibition, Environmental Aspects, and pH Control: Part II: Corrosion Control by pH Stabilization, in Corrosion 2006. 2006, NACE International: San Diego Ca. 122. Halvorsen, A.M.K., et al., The Reletionship Between Internal Corrosion Control Method, scale Contol and MEG Handling of a Multiphase Carbon Steel Pipeline Carrying Wet Gas with CO2 and Acetic Acid, in Corrosion 2007. 2007, NACE International: Nashville, Tennessee. 123. Hagerup, O. and S. Olsen, Corrosion Control by pH Stabilizer, Materials and Corrosion Monitoring in 160 km Multiphase Offshore Pipeline, in Corrosion 2003. 2003, NACE International: San Diego Ca. 124. Kvarekval, J. and A. Dugstad, Pitting Corrosion in CO2/H2S Containing Glycol Solutions under Flowing Conditions, in Corrosion 2005. 2005, NACE International: Houston, Tx. 125. N.Hackerman, E.S.S.a., NACE Basic Corrosion Course. 1970, NACE: Houston, Texas. 126. Vuorinen, E., E. Kálmán, and W. Focke, Introduction to Vapour Phase Corrosion Inhibitors in Metal Packaging. Surface Engineering, 2004. 20(4): p. 281-284. 127. B.Sanyal, Organic Compounds as Corrosion Inhibitors in Different Environments -A Review. Progress in Organic Compounds as Corrosion 1981. 9(2): p. 165-236. 128. E.Hamner, N., ed. Scope and Importance of Inhibitor Technology. Corrosion Inhibitors, ed. N. C.C. 1973, NACE: Houston, Texas. 1-6. 129. Rostami, A., Review and Evaluation of Corrosion Inhibitors Used in Well Stimulation, in SPE International Symposium on Oilfield Chemistry. 2009, Society of Petroleum Engineers: The Woodlands. Texas. 130. Crouse, M., et al., Evaluation of Potassium Permanganate (KMnO4) as a Green Corrosion Inhibitor/Sealant for Anodized Al 2024 and Al 6061 at Different pH Values, in Corrosion 2002. 2002, NACE International: Denver Co. 131. Okamoto, G., et al., Effect of Organic Inhibitors on the Polarization Characteristics of Mild Steel in Acid Solution. Corrosion Science, 1962. 2(1): p. 21-27. 132. jr, R.l.O., Theoretical Aspects of Corrosion Inhibitors and Inhibition, in Corrosion Inhibitors, N. C.C., Editor. 1981, NACE: Houston Texas. p. 7-27. 133. Meakins, R.J., Alkyl Quaternary Ammonium Compounds as Inhibitors of the Acid Corrosion of Steel. Journal of Applied Chemistry, 1963. 13(8): p. 339-345. 134. Campbell, S. and V. Jovancicevic, Corrosion Inhibitor Film Formation Studied by ATR-FTIR, in Corrosion 99. 1999, NACE International: San Antonio, Tx. 135. Hellberg, P.-E., Environmentally Acceptable Polymeric Corrosion Inhibitors, in SPE International Symposium on Oilfield Chemistry. 2011: The Woodlands, Texas, USA. 136. Mackenzie, C.D., et al., Development of a New Corrosion Management Tool - Inhibitor Micelle Presence as an Indicator of Optimum Dose, in SPE International Conference on Oilfield Corrosion, SPE, Editor. 2010: Aberdeen, UK. 137. Durnie W., D.M.R., Jefferson A., and Kinsella B., Development of a Structure-Activity Relationship for Oil Field Corrosion Inhibitor. The Electrochemical Society, 1999. 146(5): p. 1751-1756. 138. De Marco, R., et al., Persistence of Carbon Dioxide Corrosion Inhibitors. Corrosion, 2002. 58(4): p. 354-363. 139. Vijayalakshmi, P.R. and R. Rajalakshmi, Inhibition of Mild Steel Corrosion Using Aqueous Extract of Cocos nucifera L. Peduncle in Acidic Solutions and Their Adsorption Characteristics, in Corrosion 2013. 2013: Orlando, Florida. 140. Leelavathi, S. and R. Rajalakshmi, Mundulea Sericea Leaves as a Corrosion Inhibitor for Mild Steel in Acidic Solution, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 141. Nalini, D. and R. Rajalakshmi, Inhibition of Mild Steel Corrosion in the Presence of p-Nitrophenyl-2-Imidazoline, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 142. Durnie, W.H., et al., A Study of the Adsorption Properties of Commercial Carbon Dioxide Corrosion Inhibitor Formulations. Journal of Applied Electrochemistry, 2001. 31(11): p. 1221-1226. 143. Gibson, D.H., The Organometallic Chemistry of Carbon Dioxide. Chemical Reviews, 1996. 96(6): p. 2063-2096. 144. N.Hackermann, R.M.H., and R.R.Annand, Corrosion, 1962. 18. 145. Wang D., L.S., Ying Y.,Wang M, Xiao He and Chen Z., Theoretical and Experimental Studies of Structure and Inhibition Efficiency of Iimidazoline Derivatives Corrosion Science, 1999. 41: p. 1911-1919. 146. N.Hackerman, K.A.a., Effect of Molecular Size on Inhibition of Dimethylpolymethylene Ammonium Chloride. Electrochemical Society, 1969. 116(5). 147. Frenier, W.W. and D.G. Hill, Green Inhibitors - Development and Applications for Aqueous Systems, in Corrosion 2004. 2004, NACE International: New Orleans, La. 148. Taj, S., R.W. Revie, and S. Papavinasam, Development of Green Inhibitors for Oil and Gas Applications, in Corrosion 2006. 2006, NACE International: San Diego Ca. 149. Taj, S., et al., Some Natural Products As Green Corrosion Inhibitors, in Corrosion 2007. 2007, NACE International: Nashville, Tennessee. 150. E.Schaschl, Method for Evaluation and Testing of Corrosion Inhibitors. Corrosion Inhibitors, ed. C.C. Nathan. 1973, Houston, Texas: NACE. 28-41. 151. Bregman, J.I., Corrosion Inhibitors. 1963, New York: Macmillan company. 152. Bowman, J.A.K.a.C.W., ed. The Chemistry of Corrosion Inhibitors used in Oil Production,. 1984, UK Corrosion: London. 153. Free, M.L., W. Wang, and D.Y. Ryu, Prediction of Corrosion Inhibition Using Surfactants. Corrosion, 2004. 60(09). 154. Mansfeld, F., S.L. Jeanjaquet, and M.W. Kendig, An Electrochemical Impedance Spectroscopy Study of Reactions at the Metal/Coating Interface. Corrosion Science, 1986. 26(9): p. 735-742. 155. Akbar, A., Understanding the Interactions Between Corrosion Scales and Inhibitor Films in Flow conditions, in School of Mechanical Engineering. 2013, University of Leeds: University of Leeds. 156. Wong, J.E. and N. Park, Effect of Corrosion Inhibitor Active Components on the Growth of Iron Carbonate Scale under CO2 conditions, in Corrosion 2008. 2008, NACE International: New Orleans, Louisiana. 157. Wong, J.E. and N. Park, Further Investigation On The Effect Of Corrosion Inhibitor Actives On The Formation Of Iron Carbonate On Carbon Steel, in Corrosion 2009. 2009, NACE International: Atlanta, Georgia. 158. Tsui, K. and J.E. Wong, Effect Of Corrosion Inhibitor Active Components On Corrosion Inhibition In A Sweet Environment, in Corrosion 2010. 2010, NACE International: San Atonia, Texas. 159. Bikkina, C., et al., Development of MEG Regeneration Unit Compatible Corrosion Inhibitor for Wet Gas Systems, in SPE Asia Pacific Oil and Gas Conference and Exhibition. 2012, Society of Petroleum Engineers: Perth, Australia. 160. Olsen, S., et al., CO2 Corrosion Prediction Model - Basic Principles, in CORROSION 2005. 2005, NACE International: Houston, Tx. 161. Ashton, J.J.B.C. The Effect of Temperature on Conductivity Measurement. 2013; Available from: http://www.camlabworld.com/originalimages/sitefiles/Tech_papers/TempCondMeas.pdf. 162. Bevilacqua, D.M.G.a.A.C. Cation Conductivity Temperature Compensation in International Water Conference,. 1997. Pittsburgh, PA,. 163. Chen, T.-Y., A Transient Technique to Determine Solution Resistance for Corrosion Rate Measurements in Low-Conductivity Solutions, in Corrosion96. 1996, NACE International: Denver , Co. 164. Waxman, M.H. and E.C. Thomas, Electrical Conductivities in Shaly Sands-I. The Relation Between Hydrocarbon Saturation and Resistivity Index; II. The Temperature Coefficient Of Electrical Conductivity. Journal of Petroleum Technology, 1974. 26(2): p. 213-225. 165. Tanupabrungsun, T., B. Brown, and S. Nesic, Effect of pH on CO2 Corrosion of Mild Steel at Elevated Temperatures, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 166. Mishra, B., et al., Development of a Predictive Model for Activation-Controlled Corrosion of Steel in Solutions Containing Carbon Dioxide. Corrosion, 1997. 53(11). 167. Al-Fozan, A.U.M.a.S.A. Pitting Behaviour of Type 316L S.S in Arabian Gulf Seawater. 1992; Available from: http://www.swcc.gov.sa/files%5Cassets%5CResearch%5CTechnical%20Papers%5CCorrosion/PITTING%20BEHAVIOUR%20OF%20TYPE%20316L%20S.S%20INARABIAN%20GULF%20SEAWATER. 168. Azghandi, M., et al., Corrosion Inhibitive Evaluation of an Environmentally Friendly Water-Base Acrylic Terpolymer on Mild Steel in Hydrochloric Acid Media. Metallurgical and Materials Transactions A, 2013. 44(12): p. 5493-5504. 169. R.H.Petrucci, W.S.H., G.E.Herring and J.Madura, General Chemistry Principles & Modern Applications. 2006, New Jersey Prentice Hall. 170. L.Pacheco, J., F.C. Ibrahim, and R. J.Franco, Testing Requirements of Corrosion Inhibitor Qualification for Pipeline Applications, in Corrosion 2010. NACE International: San Antonio, TX. 171. Mok, W.Y., et al., Control of Localized Corrosion using Green Corrosion Inhibitors, in Corrosion 2005. 2005, NACE International: Houston Texas. 172. Frenier, W.W., F.B. Growcock, and V.R. Lopp, Mechanisms of Corrosion Inhibitors Used in Acidizing Wells. SPE Production Engineering, 1988. 3(4): p. 584-590. 173. Hu, X., I.M. Ismail, and A. Neville, Investigation of Pitting Corrosion and Inhibition in Sweet Conditions, in Corrosion 2013. 2013, NACE International: Orlando, Florida. 174. Jenkins, A., Performance of High-Temperature, Biodegradable Corrosion Inhibitors, in Corrosion 2011. 2011, NACE International: Houston, Texas. 175. Magana-Zavala, C.R., et al., Electrochemical Impedance Spectroscopy (EIS) Modelling of Different Behaviours of Ni and Ni Oxide Thin Films for Corrosion Prevention in Sour Media. Anti-Corrosion Methods and Materials, 2010. 57(3): p. 118-125. 176. Castaneda, H., E. Sosa, and M.A. Espinosa-Medina, Film Properties and Stability Influence on Impedance Distribution During the Dissolution Process of Low-carbon Steel Exposed to Modified Alkaline Sour Environment. Corrosion Science, 2009. 51(4): p. 799-806. 177. Lopez, H.C., et al., Film Stability for API 5L X-52 Line Pipe Steel in CO2 (aq) and Cl (aq) Solutions in Presence of Amine Based Inhibitor under Hydrodynamic Conditions, in Corrosion 2004. 2004, NACE International: New Orleans, Louisiana. 178. Duval, S., R. Sauvant-Moynot, and F. Ropital, EIS: A Powerful Tool for In Situ Monitoring Coating Performance, in Corrosion 2003. 2003, NACE International: San Diego, Ca. 179. Wang, H., et al., Characterization of Inhibitor and Corrosion Product Film Using Electrochemical Impedance Spectroscopy (EIS), in Corrosion 2001. 2001, NACE International: Houston, Texas. 180. Lillard, R.S., et al., Using Local Electrochemical Impedance Spectroscopy to Examine Coating Failure. Corrosion, 1995. 51(04). 181. Ruedisueli, R.L., A. Sheetz, and A. Field, Paint Coating Electrical Resistance and Performance in Service Environments, in Corrosion 2006. 2006, NACE International: San Diego, Ca. 182. Torres-Islas, A., et al., Corrosion Inhibition Efficiency Study in a Microalloyed Steel for Sour Service at 50 degrees C. Journal of Applied Electrochemistry, 2010. 40(8): p. 1483-1491. 183. Mansfeld, F., et al., Analysis of Electrochemical Impedance and Noise Data for Polymer Coated Metals. Corrosion Science, 1997. 39(2): p. 255-279. 184. Esih I., S.T.a.P.Z. Inhibition of Mild Steel Corrosion in CO2-Saturated Chloride Solutions by Acylated Polyamine Salts. in Proceedings of the 8th European Symposium on Corrosion Inhibitors (8 SEIC). 1995. Ann, Univ. Ferrara, N.S. 185. Halvorsen, E.N., et al., Qualification of Scale Inhibitors for Subsea Tiebacks With MEG Injection, in SPE International Symposium on Oilfield Chemistry. 2009, Society of Petroleum Engineers: The Woodlands. Texas. 186. Nesic, S. and K.-L.J. Lee, A Mechanistic Model for Carbon Dioxide Corrosion of Mild Steel in the Presence of Protective Iron Carbonate FilmsPart 3: Film Growth Model. Corrosion, 2003. 59(07). 187. Nesic, S., et al., A Mechanistic Model for Carbon Dioxide Corrosion of Mild Steel in the Presence of Protective Iron Carbonate Films - Part 2: A Numerical Experiment. Corrosion, 2003. 59(6): p. 489-497. 188. Llongueras, J.G., et al., Mechanism of FeCO3 Formation on API X70 Pipeline Steel in Brine Solutions Containing CO2, in Corrosion 2005. 2005, NACE International: Houston, Texas. 189. Nordsveen, M., et al., A mechanistic model for carbon dioxide corrosion of mild steel in the presence of protective iron carbonate films - Part 1: Theory and verification. Corrosion, 2003. 59(5): p. 443-456. 190. Han, J., et al., Electrochemical Investigation of Localized CO2 Corrosion on Mild Steel, in Corrosion 2007. 2007, NACE International: Nashville, Tennessee. 191. Hitoshi Shindo, a.M.K., Stabilities of Crystal Faces of Aragonite (CaCO3) Compared by Atomic Force Microscopic Observation of Facet Formation Processes in Aqueous Acetic acid. Physical Chemistry Chemical Physics, 2005. 7(4): p. 691-6. 192. Ahmad, Z., Principles of Corrosion Engineering and Corrosion Control. Materials & Mechanical. 2006: Butterworth-Heinemann. 1-672. 193. Hong, T., et al., EIS Study of Corrosion Product Film in Pipelines, in Corrosion 2000. NACE International: Orlando, Florida. 194. Gulbrandsen, E. and J.H. Morard, Study of the Possible Mechanisms of Steel Passivation in CO2 Corrosion, in Corrosion 99. 1999, NACE International: San Antonio, Tx. 195. Riemenschneider, W. and H.M. Bolt, Esters, Organic, in Ullmann's Encyclopedia of Industrial Chemistry. 2000, Wiley-VCH Verlag GmbH & Co. KGaA. 196. Ismail, I.M., Inhibition of Pitting on Carbon Steel, in School of Mechanical Engineering. 2011, University of Leeds: University of Leeds. 197. Alink, B.A., et al., Mechanism of CO2 Corrosion Inhibition by Phosphate Esters, in Corrosion99. 1999, NACE International: San Atonia, Texas. 198. Sun, W., K. Chokshi, and S. Nesic, Iron Carbonate Scale Growth and the Effect of Inhibition in CO2 Corrosion of Mild Steel. 2005, NACE International. 199. Nyborg, R., et al., Effect of Steel Microstructure and Composition on Inhibition of CO2 Corrosion, in Corrosion 2000. 2000, NACE International: Orlando, Fl. 200. Kvarekval, J., S. Skjerve, and S. Olsen, The Effect of O2 on CO2 Corrosion in pH Stabilized Gas/Condensate Pipelines, in Corrosion 2005. 2005, NACE International: Houston, Tx. 201. Lu, H., A.T. Kan, and M.B. Tomson, Effects of Monoethylene Glycol on Carbonate Equilibrium and Calcite Solubility in Gas/Monoethylene Glycol/Water/Salt Mixed Systems, in SPE International Symposium on Oilfield Chemistry. 2009, Society of Petroleum Engineers: The Woodlands. Texas. 202. Vuppu, A.K. and W.P. Jepscm, Study Of Sweet Corrosion In Horizontal Multiphase, Carbon Steel Pipelines, in OTC 1994, Offshore Technology Conference: Houston, Texas. 203. Nordsveen, M., S.N.R. Nyborg, and A. Stangeland, A Mechanistic Model for Carbon Dioxide Corrosion of Mild Steel in the Presence of Protective Iron Carbonate FilmsPart 1: Theory and Verification. Corrosion, 2003. 59(05). 204. Han, J., B.N. Brown, and S. Nesic, Investigation of the Galvanic Mechanism for Localized Carbon Dioxide Corrosion Propagation Using the Artificial Pit Technique. Corrosion, 2010. 66(9). 205. Berntsen, T., M. Seiersten, and T. Hemmingsen, Effect of FeCO3 Supersaturation And Carbide Exposure On the CO2 Corrosion Rate of Carbon Steel, in Corrosion 2011. 2011, NACE International: Houston, Texas."],"dcterms:accessrights":["public"],"dc:title":["Corrosion processes and mechanisms in the presence of MonoEthylene Glycol (MEG)"],"dc:type":["Thesis"],"dc:type.qualificationlevel":["doctoral"],"dc:type.qualificationname":["Ph.D"]},"updated_at":"2026-11-18T21:28:19Z"}